Abstract

We explore the U-Ge phase diagram using thin film growth by co-deposition of U and Ge via d.c. magnetron sputtering. Using three different single crystal substrates - MgO, CaF2_2 and SrTiO3_3 - we have stabilised mixed phase films of mostly UGe3_3 and UGe, with evidence of UGe2_2 as well. At higher temperatures UO2_2 forms as a consequence of gettering of oxygen from several types of substrate. Several UGe3_3 dominated samples grown on MgO substrates have also been characterised electrically, showing residual resistivity ratios up to six.

Introduction

Binary compounds incorporating uranium display a wide range of physics, from metallic ferromagnetism and antiferromagnetism in UH3UH_{3} [1] and UNUN [2], respectively, to exotic superconductivity and heavy fermion character in systems such as UPt3UPt_{3} [3] and UGe2UGe_{2} [4], to name but a few examples. In this context the materials science of their diverse crystal structures is of great interest. In bulk many of these systems have been studied in detail, but far less work has been done on thin film systems [5]. Thin films not only offer the potential to create idealised surfaces for study, but possess a range of tuning parameter that can be used to control the structural, magnetic and electronic properties of materials, such as the dimensionality (via film thickness), substrate strain and proximity with other materials [6].

Following a recent study of thin film epitaxial growth of UU-SiSi materials [7], here we study the UU-GeGe binary system, motivated by the possibility of stabilizing phase-pure single crystal thin films of UGe2UGe_{2} to ultimately allow the study of its unconventional superconductivity, magnetism, quantum criticality and heavy fermion behavior. To achieve successful epitaxial thin film growth of materials whose binary phase diagrams have a range of line compounds, appropriate single crystal substrates need to be identified. These should provide a suitable lattice match to the desired phase, as well as being chemically compatible - minimizing interdiffusion or chemical reactions between the film and substrate during growth, which is often required to be at elevated temperatures to obtain good crystallinity. Additionally, a key challenge is to find substrates and growth conditions that promote the formation of one phase.

Before introducing the experimental methods, we briefly discuss the various crystal structures and electronic properties in U-Ge phase diagram, compare with the U-Si system, and show some possible lattice matches with several common commercial single crystal substrates. The U-Ge binary phase diagram consists of five different phases namely: U5Ge4U_5Ge_4, UGeUGe, U3Ge5U_3Ge_5, UGe2UGe_2 and UGe3UGe_3 in order of increasing Ge content. These are summarised in Table 1, which also shows the symmetries and lattice parameters of these phases. We note that the original phase diagram by Lyahsenko & Bykov [8] included U7GeU_7Ge and U3Ge4U_3Ge_4 phases which were later corrected to U3Ge5U_3Ge_5 and UGeUGe. Compared to the U-Si system, the line compounds are slightly different in stoichiometry. In the U-Si case there are the following phases: U3SiU_3Si, U3Si2U_3Si_2, USiUSi, U3Si5U_3Si_5, USi2USi_2 and USi3USi_3 in order of increasing Si content [9]. Given the smaller Si atom compared to Ge, the U-Si bond length is shorter than the U-Ge bond length, leading to a stronger 5f5f–ligand hybridisation in the silicides, meaning that the electrons are more itinerant in U-Si phases compared to U-Ge which are more localised.

PhaseStructureSpace groupaa (Å)bb (Å)cc (Å)Reference
U5Ge4U_5Ge_4HexagonalP63/mcmP6_3/mcm8.7448.7445.863[11]
UGeUGeOrthorhombicPbcm9.8278.9325.841[12]
U3Ge5U_3Ge_5HexagonalP6/mmmP6/mmm3.9543.9544.125[13]
UGe2UGe_2OrthorhombicCmmm3.99715.0394.087[4]
UGe3UGe_3CubicPm3ˉmPm\bar{3}m4.2064.2064.206[14]

Table 1. Different phases present in the U-Ge binary phase diagram, together with crystal symmetries, space groups and lattice parameters (aa, bb and cc). Phases are listed in order of increasing Ge content, from top to bottom.

As a consequence, several of the U-Ge compounds are magnetic. For example a ferromagnetic transition at 94 K, is found in U3Ge5U_3Ge_5. This difference can also be framed in the Hill limit picture [10], since the shortest distance U–U bond length, dU−Ud_{\mathrm{U-U}}, in U3Ge5U_3Ge_5 is 3.95 Å which is well above the Hill limit of 3.4 Å. Following a similar argument dU−U∼3.84d_{\mathrm{U-U}} \sim3.84 Å for UGe2UGe_2, also places it in the localised electron behaviour region, consistent with the observed ferromagnetic state. In the case of the U-rich germanides, both U5Ge4U_5Ge_4 and UGeUGe exhibit paramagnetic behaviour down to 2 K, with dU−U∼2.9d_{\mathrm{U-U}} \sim2.9 Å placing them well below the Hill limit.

Focusing on the UGe2UGe_2 system, although the system is formally orthorhombic, the aa and cc lattice parameters differ only by ∼2%\sim2\%, giving the possibility of a relatively simple ‘cube-on-cube’ epitaxial relationship with common cubic substrates. Two examples are shown in Figure 1, where matches with SrTiO3_3 (STO) {100}\{100\} and MgO {100}\{100\} surfaces are schematically shown. In the case of STO, (lattice parameter a=3.906a = 3.906 Å) there would be a −2.3% strain (compressive) for the aa direction of UGe2_2, and a +4.7% strain (tensile) in the cc direction, assuming coherent growth. Here the mismatch has been defined as 100% ×(afilm−asubstrate)/asubstrate\times(a_{\mathrm{film}} - a_{\mathrm{substrate}})/a_{\mathrm{substrate}}. For MgO (lattice parameter a=4.213a = 4.213 Å) the strains are ∼ +3% and +5% (both tensile) for cc and aa, respectively. The lattice mismatch between cubic UGe3_3 and these two substrates assuming a cube-on-cube epitaxial relationship is also relatively small for the MgO in particular (+0.17%), and −7.7% for STO. These possible matches motivated this study. Finally we note the {100}\{100\} surfaces of CaF2_2 (lattice parameter a=5.462a = 5.462 Å). While not as well-matched to the various U-Ge phases for simple epitaxial relationships, we also used CaF2_2 in this work as a comparison, since it lacks oxygen in its structure. As will be subsequently shown in this work, the oxygen can be gettered by the U-containing film from the substrates during growth at elevated temperatures, leading to unwanted oxide phases.

Possible epitaxial matches between UGe2 on SrTiO3 and MgO surfaces

Figure 1. Possible epitaxial matches between UGe2_2 on the {100}\{100\} surfaces of SrTiO3_3 (STO, top) and MgO (bottom). Lattice directions aa and cc are shown for UGe2_2. Images created using VESTA [15].

Experimental Methods

All samples in this study were grown using the dedicated ‘FaRMS’ actinide d.c. magnetron sputtering capability at the University of Bristol, UK [16]. This ultra-high vacuum system operates at base pressures ∼10−10\sim10^{-10} mbar and contains four sputtering guns inside a load-locked chamber. Substrates are loaded onto an adjustable height stage adjacent to a Ta resistive heater capable of achieving temperatures of up to 850 °C. Samples were fabricated by co-sputtering from separate U and Ge targets in presence of Ar at a pressure of 7.3×10−37.3 \times10^{-3} mbar. Deposition rates for U and Ge were individually calibrated by ex-situ x-ray reflectivity measurements. Typical deposition rates were 0.03–0.06 nm/s, and were tuned by varying the power supplied to each target in the range 12–30 W for Ge, with the U gun power held at 10 W. Nominally for a 1:2 U:Ge ratio the estimated required power ratio was also 1:2. For samples grown above room temperature (RT), the substrates were held at the growth temperature, TgT_{\mathrm{g}}, to within an error of ±25\pm25 °C. Film thicknesses were nominally ∼50\sim50 nm for all samples. A polycrystalline Nb cap, of thickness ∼9\sim9 nm was grown in-situ on all samples after cooling the samples to ambient temperature, to prevent oxidation in air.

Three types of commercial cubic single crystal substrate were used for growth: CaF2_2, SrTiO3_3, and MgO. All substrates were purchased from Crystal GmbH, had dimensions 10 mm ×\times 10 mm ×\times 0.5$ mm, were oriented with a <100><100> direction normal to the substrate plane, and were polished to optical grade. Table 2 summarises the samples fabricated in this study. X-ray diffraction (XRD) experiments were carried out at room temperature with a laboratory based Cu-Kα\alpha source to determine the U-Ge phases present in the samples, as well as their crystallographic orientation in the specular direction. Temperature-dependent transport measurements were carried out in a liquid helium-4 dip probe, in a four-point resistance geometry, using a d.c. bipolar bias current method with current magnitude of the order of 100 μ\muA.

Results & Discussion

Temperature series on SrTiO3

Samples were grown at three values of TgT_{\mathrm{g}}: RT, 300 °C and 525 °C, at constant sputtering power onto STO {100}\{100\} substrates. The sample grown at RT showed no significant peaks in the XRD measurement other than those associated with the substrate and the data are not shown. 2θ−ω2\theta-\omega XRD scans for the two samples grown at higher TgT_{\mathrm{g}} are shown in Figure 2. For the sample grown at Tg=300T_{\mathrm{g}} = 300 °C reflections from two U-Ge phases (UGe3_3 and UGe) were identified, with two dominant different orientations present for UGe3_3, and one for UGe. When TgT_{\mathrm{g}} was raised to 525 °C, several changes to the XRD data are clear. Firstly UO2_2 peaks start to appear particularly associated with reflections from the (200) plane with some lower intensity peaks related to reflections from (111) planes. The UGe phase is no longer present, and additionally elemental Ge and Nb reflections are observed.

Figure 2. Specular XRD measurement of U-Ge thin films grown on STO for Tg=300 ∘CT_g = 300\,^\circ\mathrm{C} (top) and 525 ∘C525\,^\circ\mathrm{C} (bottom). Indexed planes are colour-coded according to the corresponding material. Lines are a guide to the eye.

Several of these observations are linked. STO is well known to be sensitive to loss of oxygen at elevated temperatures and in vacuum (e.g. [17]), and we therefore conclude that the oxygen required to form UO2_2 originates from the STO substrate. This in turn reduces the

SubstrateSample IDPower (W) UPower (W) GeTgT_g (°C)
STOSN-11020RT
STOSN-21020300
STOSN-31020525
MgOSN-41020RT
MgOSN-51020300
MgOSN-61020525
MgOSN-71020775
MgOSN-81020850
MgOSN-91015850
MgOSN-101012850
CaF2_2SN-111030525
CaF2_2SN-121025525
CaF2_2SN-131020525
CaF2_2SN-141017525

caption: Summary of samples grown on various substrates with varying growth temperatures, TgT_g, and sputtering powers.

:::

amount of readily available U-atoms to form U-Ge compounds, reducing the UGe component. With the loss of the U-atoms to form U-Ge phases, the excess Ge atoms crystallises in its elemental form. It should also be highlighted that although both samples contained UGe3_3 phases, the higher temperature sample showed that the phase is {100} textured. Finally we note that the Nb (110) peak is visible in the higher temperature sample only since the (111) UGe3_3 Bragg peak obscures the signal in the lower TgT_g sample.

Temperature and power series on MgO

Motivated by the epitaxial USi2_2 film grown on MgO substrates, and the potential epitaxial match discussed above, five U-Ge samples were grown at temperatures varying between RT up to Tg=850T_g = 850 °C. The same U:Ge sputtering power ratio was used as for the STO samples, as well as an additional two samples at Tg=850T_g = 850 °C with varying Ge sputtering power.

First we focus on the four lower TgT_g samples. The 2θ−ω2\theta-\omega XRD scans for these samples are shown in Figure 3. As for the samples grown on STO, the RT grown sample showed no Bragg peaks (data not shown). Also at the highest of these four growth temperatures, Tg=775T_g = 775°C, Bragg peaks corresponding to UO2_2 (200) were observed. Again both UGe and UGe3_3 phases were observed. The UGe3_3 phase showed (100) texture when TgT_g was increased to 775°C, with the (111)(111) orientation observed at lower TgT_g. However in the case of the samples grown on MgO substrates there was no evidence of crystalline elemental Ge, which was observed in the STO series.

Figure 3. High angle XRD measurement of U\mathrm{U}:Ge\mathrm{Ge} thin films grown on MgO\mathrm{MgO} with varying temperatures. Indexed planes are colour-coded according to the corresponding material. At higher temperatures, as in the case of STO\mathrm{STO}, UO2\mathrm{UO}_{2} peaks start to appear. Stars indicate peaks that could not be indexed to any expected phases.

A relatively weak signal from the UGe2\mathrm{UGe}_2 phase can also be observed for the sample grown on MgO at ∼775 ∘C\sim775\,^\circ\mathrm{C}. Increasing TgT_g from ∼525 ∘C\sim525\,^\circ\mathrm{C} to 775 ∘C775\,^\circ\mathrm{C} suppresses the UGe phase, similar to what was observed using the STO substrate. For the sample grown at 775 ∘C775\,^\circ\mathrm{C} assuming a cubic lattice for UGe3\mathrm{UGe}_3, using the specular (100)(100) and (300)(300) Bragg peaks at 21.17∘21.17^\circ and 66.85∘66.85^\circ respectively, and dhkl=a/h2+k2+l2d_{hkl} = a/\sqrt{h^2+k^2+l^2}, the lattice parameter can be estimated to be a=4.197a = 4.197 Å, close to the bulk value.

In addition to the coupled scan presented, an ω\omega scan provides information on the crystal mosaicity or tilt disorder, as well as the presence of strain, defects, or asymmetric domain distributions in the system. For the sample grown at 775 ∘C775\,^\circ\mathrm{C} on MgO, the full width at half maximum (FWHM) of the (100)(100) UGe3\mathrm{UGe}_3 peak was 0.46±0.01∘0.46 \pm0.01^\circ, (the FWHM of the (200)(200) MgO substrate peak was 0.091±0.001∘0.091 \pm0.001^\circ), indicating good crystallinity of the film. For this

Figure 4. ω\omega scan comparison of UGe3_3 (100) and MgO (200) peaks for sample SN-7. Open circles are the data and the solid lines are best fits using the Voigt function. UGe3_3 data are offset vertically for clarity.

sample, off-specular XRD scans were conducted to investigate the in-plane matching with the substrate, as shown in Figure 5 for the {310}\{310\} reflection family of UGe3_3. For a bulk single crystal of UGe3_3 with the fcc structure, one would expect to see a 4-fold symmetry in a 360∘360^\circ rotation in ϕ\phi. These peaks should be symmetric and have a periodicity of Δϕ=90∘\Delta\phi= 90^\circ between each peak. In fact the off-specular scan shows eight distinct peaks alternating in ϕ\phi between relatively high and low intensity. These two sets of peaks indicate the presence of a major domain and a minor domain of UGe3_3 rotated 45∘45^\circ with respect to each other. Given the discussion at the beginning of this paper on the possible good epitaxial match with this substrate, the formation of UGe3_3 on MgO with a cube-on-cube match was predicted, but the minor domains rotated by 45∘45^\circ were not expected.

Pole figure data for the {310} reflections of UGe$_3$ for sample SN-7

Figure 5. Pole figure data for the {310}\{310\} reflections of UGe3_3 for sample SN-7.

To further study the U:Ge thin phases on the MgO substrates, a power series study was conducted at a slightly higher temperature of 850∘850^\circC, with variable Ge sputtering power and fixed U sputtering power (see the growth details in Table 2). The specular XRD scans of these samples are shown in Figure 6. In all three XRD scans there is clear evidence of the UGe3_3 phase, with several different growth orientations for the highest Ge power, but with UGe3_3 (100) reflections present for all three samples. The formation of UO2_2 is also clear in the XRD data with (200), (400) and (111) peaks all observable, consistent with the observations for the Tg=775T_{\mathrm{g}} = 775 °C sample, SN-7. Similar to sample SN-3 grown on STO (although at a higher TgT_{\mathrm{g}}), here we again find peaks corresponding to elemental Ge in the specular scans in all three samples. It is also notable that the reduction in Ge sputtering power does not drive the formation of UGe phase. As we will see in the next section such a trend does occur when CaF2_2 substrates were used.

Figure 6. High angle measurement of U:Ge thin films grown on MgO at ∼850 ∘C\sim850\,^\circ\mathrm{C} with varying Ge sputtering power indicated in the top left of each panel. Indexed planes are colour-coded according to the corresponding material. At lower Ge power, relatively stronger elemental Ge peaks become visible while UGe3_3 peaks are suppressed. Stars indicate peaks that could not be indexed to any expected phases.

CaF2_2 substrate

Finally in this section we discuss the XRD characterisation of the samples grown on (100) CaF2_2 substrates, which were deposited at the same Tg=525T_{\mathrm{g}} = 525 °C with a range of Ge sputtering powers. The normalised XRD data for these samples are shown in Figure 7. Note that the (200) CaF2_2 substrate reflection at ∼32.76∘\sim32.76^\circ cannot be seen here since an ω\omega angle offset was introduced to reduce the substrate peak intensity, making it easier to analyse the other features in the dataset. For the sample with the highest Ge content (SN-11), the major Bragg peaks observed are indexed to UGe3_3 with (110) texture. On the other hand, sample

Figure 7. Specular XRD measurements of U-Ge thin films grown on CaF2_2 with varying Ge growth power. The data have been normalised and offset vertically for clarity. Ge content decreases from top to bottom. Colour-coded vertical lines at the bottom show the literature peak positions for the various reflections for the different phases present in the films.

SN-14, grown with the lowest Ge power shows stronger Bragg peaks from the (211) plane of UGe. This is consistent with the reduction in Ge content in these thin films moving across the phase diagram. In the case of samples SN-12 and SN-13, grown with intermediate Ge power, both UGe and UGe3_3 phases are present. On closer inspection, there is also a texture change: the UGe3_3 phases show (100) texture in these two samples instead of (110) seen in the Ge-richer sample. Additionally, it can also be seen that between the two mixed-phase samples, the Ge-poorer sample (SN-13), indicates the transition point where the (211) UGe peaks clearly starts to appear alongside the (100) UGe3_3 peak seen. No other U-Ge phases were observed in these samples.

To quantify the mosaicity and crystallinity of the samples, ω\omega XRD scans were made on selected UGe3_3 and UGe reflections. These ω\omega scans are shown in Figure 8. After fitting Voigt functional forms to the data, the resultant FWHM of the peaks are summarised in Table 3. Firstly, focusing on the (100) UGe3_3 peak, we can see that the FWHM decreases with decreasing Ge power indicating a reduction in crystallinity. For the (110) UGe3_3 peak the 30 W sample (SN-11) has the best crystallinity of the series. Interestingly for this sample,

Figure 8. ω\omega scan on selected UGe3_3 and UGe peaks for samples grown on CaF2_2 with various Ge powers. a) (100) UGe3_3, b) (211) UGe, c) (110) and d) (111) UGe3_3 peaks. The plots have been arranged in order of decreasing Ge power with the same colour code representing the samples as in the coupled scan shown in Figure 7.

Sample IDGe Power (W)FWHM (∘^\circ)
SN-1130(100) UGe3_31.32±0.03∘1.32 \pm0.03^\circ(211) UGe−-(110) UGe3_31.43±0.01∘1.43 \pm0.01^\circ(111) UGe3_3−-
SN-1225(100) UGe3_31.94±0.03∘1.94 \pm0.03^\circ(211) UGe−-(110) UGe3_33±1∘3 \pm1^\circ(111) UGe3_32.3±0.9∘2.3 \pm0.9^\circ
SN-1320(100) UGe3_32.2±0.1∘2.2 \pm0.1^\circ(211) UGe2.83±0.3∘2.83 \pm0.3^\circ(110) UGe3_32.4±0.1∘2.4 \pm0.1^\circ(111) UGe3_32.1±0.5∘2.1 \pm0.5^\circ
SN-1417(100) UGe3_3−-(211) UGe2.52±0.07∘2.52 \pm0.07^\circ(110) UGe3_3−-(111) UGe3_3−-

caption: tbl:3: FWHM values for selected peaks of UGe3_3 and UGe thin films grown on CaF2_2 calculated based on the Voigt functional fits made to the ω\omega scans of (100), (110) and (111) UGe3_3 peaks and the (211) UGe peak.

:::

while we see an improvement in the texture compared to the other samples, we did not observe an improved rocking curve. When focusing on the (211) UGe peak, the coupled scan FWHM clearly improves for the lower Ge power (i.e. moving from the sample grown at 20 W to the sample grown at 17 W). This change is also reflected in the ω\omega scan: a slightly narrower FWHM peak. Finally we note that the (111) reflection of UGe3_3, when visible (only for the two intermediate growth powers) reveal little difference in crystallinity to within the measurement error.

Resistivity measurements

Figure 9. Resistance-temperature measurements on selected UGe thin films. a) Sample SN-7 grown on MgO [1], which showed majority UGe3_3 peaks. b) SN-11 grown on CaF2_2 [1], which showed majority UGe3_3 peaks. c) Sample SN-14, grown on CaF2_2 [1], which showed strong UGe peaks. Blue arrow in (c) indicates a distinct kink in the R(T)R(T) data. Residual resistance ratios (RRRRRR) are shown in each panel.

In addition to the XRD measurements presented, some longitudinal resistance versus temperature (R(T)R(T)) measurements were performed on three selected samples as shown in 9. These measurements were performed a He-4 dip probe, in a temperature range of 4.2 K ≤T≤\le T \le 290 K. Firstly all the samples showed metallic behaviour with a rather linear R(T)R(T) at higher temperatures. As a measure of the quality of the samples, we show the residual resistance ratio (RRRRRR), given by RRR=R(T=295K)/R(T=4.2K)RRR = R(T = 295\mathrm{K})/R(T = 4.2\mathrm{K}). Comparing the two UGe3UGe_3 samples, the sample grown on the MgO substrate showed a larger RRR∼6.1RRR \sim6.1 in comparison to the sample grown on CaF2CaF_2 with RRR∼3.1RRR \sim3.1, consistent with the narrower rocking curve of the UGe3UGe_3 peaks for the sample grown on the MgO substrate. Note that bulk UGe3UGe_3 does not show any particular magnetic ordering down to 2 K, so the featureless R(T)R(T) plots are consistent with this. On the other hand the R(T)R(T) for the sample with the majority UGeUGe phase shows a distinct change in the slope of the R(T)R(T) at around ∼74\sim74 K which possibly indicates the onset of some spin fluctuations, consistent with previous specific heat measurements that have indicated a larger specific heat coefficient γ(0)\gamma(0) value for UGeUGe in comparison to the other germanides [18]. Overall however, it is clear that the MgO substrate gives rise to the highest quality UGe3UGe_3 films, and further thicknesses are required to understand if surface scattering is limiting the value of RRRRRR, or whether scattering due to the phase impurities is more dominant.

Summary and conclusions

In conclusion we have stabilised a range of crystalline binary U-Ge phases on various substrates using thin film growth at a range of growth temperatures and sputtering powers. Although we have been unable to stabilise single phase material so far, we have observed dominant growth of UGe3UGe_3 and UGeUGe phases by varying the substrate material and growth conditions. Majority UGe2UGe_2 phase thin films have so far proved illusive. A notable challenge was the emergence of oxide phases at higher growth temperatures due to gettering by the U of oxygen in the substrate material. Future studies should examine the possibility of buffer layers between the substrate and the U-Ge layers that can simultaneously act as a diffusion to oxygen migration, as well as providing further degrees of freedom for epitaxial matching and phase stabilisation. We note after the completion of this work, related spectroscopic studies of U-Ge samples were published elsewhere [19].

Acknowledgements

We acknowledge the funding and support from the UKRI Engineering and Physical Sciences Research Council (EPSRC), UK. In particular this work utilised the National Nuclear User Facility FaRMS, grant: EP/V035495/1. We thank P. Babu and Z. Huang for early help in this project, and R. Nicholls for insightful comments.

References

  1. [1]R. Troć and W. Suski. The discovery of the ferromagnetism in U(H,D)₃: 40 years later. Journal of Alloys and Compounds, 219:1–5, 1995.DOI
  2. [2]N. A. Curry. An investigation of the magnetic structure of uranium nitride by neutron diffraction. Proc. Phys. Soc., 86:1193, 1965.DOI
  3. [3]R. Joynt and L. Taillefer. The superconducting phases of UPt₃. Reviews of Modern Physics, 74(1):235–294, 2002.
  4. [4]S. S. Saxena, P. Agarwal, K. Ahilan, F. M. Grosche, R. K. W. Haselwimmer, M. J. Steiner, E. Pugh, I. R. Walker, S. R. Julian, P. Monthoux, G. G. Lonzarich, A. Huxley, I. Sheikin, D. Braithwaite, and J. Flouquet. Superconductivity on the border of itinerant-electron ferromagnetism in UGe₂. Nature, 406(6796):587–592, 2000.
  5. [5]R. Springell, E. Lawrence Bright, D. A. Chaney, L. M. Harding, C. Bell, R. C. C. Ward, and G. H. Lander. A review of uranium-based thin films. Advances in Physics, 71(3-4):87–165, October 2022.arxiv.org/abs/2307.01018
  6. [6]S. Chatterjee. Heavy fermion thin films: progress and prospects. Electronic Structure, 3(4), 2021.DOI
  7. [7]L. M. Harding, E. Lawrence Bright, J. Laverock, D. T. Goddard, and R. Springell. Epitaxial stabilisation of uranium silicide line compounds. Thin Solid Films, 768:139690, 2023.DOI
  8. [8]V. N. Lyashenko V. S., Bykov. An investigation of the alloys of the uranium-germanium system. The Soviet Journal of Atomic Energy, 8:132–134, 1961.DOI
  9. [9]S. C. Middleburgh, R. W. Grimes, E. J. Lahoda, C. R. Stanek, and D. A. Andersson. Non-stoichiometry in U₃Si₂. Journal of Nuclear Materials, 482:300–305, 2016.DOI
  10. [10]H. H. Hill. Early actinides: the periodic system’s f electron transition metal series. Nucl. Met., Met. Soc. AIME, 17:2–19, 1970.
  11. [11]P. Boulet, M. Potel, J. C. Levet, and H. Noël. Crystal structure and magnetic properties of the uranium germanide U₅Ge₄. J. of Alloys and Comp., 262:229–234, 1997.DOI
  12. [12]R. Troć, N. Henri, and P. Boulet. Magnetotransport of compounds in the U–Ge system. Philosophical Magazine B, 82(7):805–824, 2002.
  13. [13]P. Boulet, M. Potel, G. André, P. Rogl, and H. Noël. Crystal and magnetic structure of the binary uranium germanide U₃Ge₅. Journal of Alloys and Compounds, 283(1-2):41–44, 1999.DOI
  14. [14]G. H. Lander, J. F. Reddy, A. Delapalme, and P. J. Brown. Magnetization density in paramagnetic UGe₃. J. Magn. and Magn. Mater., 14(2-3):295–297, 1979.DOI
  15. [15]K. Momma and F. Izumi. Vesta 3 for three-dimensional visualization of crystal, volumetric and morphology data. J. Appl. Cryst., 44:1272, 2011.DOI
  16. [16]https://nnuf-farms.bristol.ac.uk/.
  17. [17]A. Spinelli, M. A. Torija, C. Liu, C. Jan, and C. Leighton. Electronic transport in doped SrTiO₃: Conduction mechanisms and potential applications. Phys. Rev. B, 81:155110, 2010.DOI
  18. [18]A. Pikul, R. Troć, A. Czopnik, and H. Noël. Low-temperature specific heat of uranium germanides. Journal of Magnetism and Magnetic Materials, 360:217–221, June 2014.DOI
  19. [19]S. G. Alex, Oleksandr Romanyuk, Ivan Zorilo, A. Andreev, F. Huber, T. Gouder, P. Malinský, A. B. Shick, and E. A. Tereshina-Chitrova. Electronic structure of UGe₂±ₓ thin films from photoelectron spectroscopy. arXiv:2601.03902, 2026.DOI

Paper details

vlnc:W_yxfpqd5s
Version
v1 · latest
Published
Fresh — added to the Hub within the last 30 days
Added
License
CC BY 4.0
Usage

views · 0

downloads · 0

A view counts once per browser per day, a download each time the PDF is requested.

  • Physics and Astronomy

Not recorded for this paper

View statement
Looking for related papers…
Contents