Electrical measurement of the Spin Hall Effect isotropy in a ferromagnet

Abstract

The spin-dependent transport properties of paramagnetic metals are roughly invariant under rotation. By contrast, in ferromagnetic materials the magnetization breaks the rotational symmetry, and thus the spin Hall effect is expected to become anisotropic. Here, using a specific design of lateral spin valves, we measure electrically the spin Hall Effect anisotropy in NiCu and NiPd, both in their ferromagnetic and paramagnetic phases. We show that the appearance of the ferromagnetic order does not lead to a sizeable anisotropy of the spin charge interconversion in these materials.

Spintronics is primarily based on the exchange interaction between the spins of conduction electrons and the local magnetization in ferromagnets (FMs). This interaction is fundamental in effects such as the Giant Magnetoresistance [1] and the Spin Transfer Torque [2]. More recently, the use of Spin Orbit (SO) interactions to manipulate spins in non-magnetic (NM) materials has triggered the birth of spinorbitronics, a new subfield of research and technology aimed at developing new spintronics devices based on SO effects, such as the SOT-MRAM [3] or the MESO devices [4].

The main SO effect used in spinorbitronics is the Spin Hall Effect (SHE) [5], that allows the conversion of a spin current into a charge current. So far, the study of the SHE has been mostly focused on non-ferromagnetic systems, such as semiconductors [6] and heavy metals [5]. Recent experiments and theoretical calculations have however shown that beyond their usual role for spin current injection [7, 8] and detection [1, 8, 24, 26] through exchange coupling, FMs possess an interesting potential for spin-charge interconversion [9, 10, 11, 12, 13]. The presence of the magnetization in these materials raises a fundamental question, as it breaks the rotational symmetry [14]. The SHE in FMs is therefore expected to be anisotropic, i.e., it should depend on the relative orientation between the magnetization and the applied charge current [15].

The rare observations of this anisotropy have been made in 3d elements below the Curie temperature, but show different results for similar materials, with a moderate anisotropy in Py [16], a large one in CoFe [17], and an isotropic behaviour in Co [18]. This could result from differences in-between material properties, but also from the fact that a precise measurement of this anisotropy remains challenging. The main techniques used to measure the SHE in heavy metals are spin pumping [19], local [20] and non-local [21] transport in nanostructures, Spin Hall Magnetoresistance [22], Spin Seebeck effect [23] and Spin-Orbit torque techniques such as ST-FMR [24] or second harmonic [25]. Observing the SHE anisotropy in FMs using these methods is however not straightforward, as it requires controlling independently the magnetization of two different FMs in direct contact [18, 28, 29, 30, 31, 32]. Techniques involving a charge current flowing into the FM-SHE material are made complicated by contamination from spurious effects such as the Planar Hall effect [33] and Anomalous Hall Effect (AHE) [34], while the methods based on non-local magnon transport that allowed for the observation of an anisotropic SHE in FMs [16, 17] involve the direct contact between the magnetic insulator and the studied FM material, which could render complex the interpretation of these results [27].

Here, we propose a new design of lateral spin valves, which provides a way to measure the anisotropy of the SHE in FMs. We use it to measure this anisotropy in NiCu and NiPd, which have been found to exhibit spin Hall angles (i.e., the charge to spin conversion rate) similar to those of the best heavy metals [28, 45, 52]. The low Curie temperature of these materials allow performing the measurements either in the paramagnetic or ferromagnetic phase. In both cases, the measured inverse spin Hall effect signal is found to be independent from the magnetization direction, the observed variations being smaller than our measurement precision of 10%. These results demonstrate that in these materials the breaking of symmetry due to the ferromagnetic order does not lead to a significant anisotropy of the SHE.

The measurements are based on the injection of a charge current from the injecting CoFe electrode towards one branch of the copper channel (cf. Figure 1b). This creates a pure spin current flowing towards the detecting electrode (Figure 1a). The device can be studied using two different measurement configurations. The non-local (NL) spin signal configuration consists in detecting the voltage drop in between the detecting electrode and the channel. By reversing the magnetization of the injecting electrode, using an external magnetic field along the easy magnetization axis, it is possible to change the polarization direction of the spin current. This leads to two different non-local voltages, high (1) and low (2), at the detecting electrode (Figure 1e). By comparing this signal with that of a device with absorber (Figure 1c and 1f), it allows measuring the spin current flowing towards the absorber [35]. It is then possible to use the ISHE measurement configuration (Figure 1d), in which the spin current is partly absorbed by the SHE absorber. The polarization of the absorbed spin current is along XX, whereas the absorbed spin current direction flows along ZZ axis. It thus generates in the ferromagnetic SHE absorber an electric field, along YY, and consequently an ISHE signal at the extremities of the absorber.

Image not extracted

Figure 1. (a) Device geometry, with the FM parts in gray, and the Cu in orange. The black arrows in the FM parts represent the magnetization directions. The dark blue and green arrows within the channel represent the spin current flow direction and its polarization, respectively. The LSV has been represented with the FMs on top for the sake of clarity, but in the actual device they lie below the Cu channel to ensure well-defined micromagnetic configurations within the electrodes and in the absorber. (b) Colored SEM image of a reference LSV without absorber, in the NL measurement configuration. (c) Colored SEM image of a LSV with absorber, in the NL measurement configuration. (d) Colored SEM image of a LSV in the ISHE measurement configuration. (e) NL signal at 12 K for a reference LSV and (f) with a 100 nm wide NiCu absorber.

When applying small fields along XX, the magnetization of the ferromagnetic SHE absorber rotates, while the magnetization of the electrodes remain along XX. It is thus possible to control the angle in between the polarisation direction of the absorbed spin current, and the magnetization of the absorber [53]. Then, if one applies large enough magnetic fields along XX, the magnetization of the injecting electrode reverses. The polarization of the injected spin current is then reversed. This causes a sign change of the ISHE signal/spin signal, allowing to measure the ISHE/spin signal amplitude.

The main advantage of this detection scheme with respect to methods based on LSVs [9, 36] is the possibility to control independently the magnetization direction of the electrodes and of the absorber, moreover using very small fields, in order to avoid field-induced contributions such as the Hall or Hanle effects [37, 38].

We used CoFe injecting and detecting electrodes, and Cu for the copper channel, in order to take advantage of its long spin diffusion length and small interface resistance with CoFe [8, 39]. A control sample has also been realised using a platinum absorber [53], as Pt is a well known material [40]. Then, the measurements of the SHE anisotropy were performed in devices with absorbers made of NiCu and NiPd. As these materials are paramagnetic at room temperature and ferromagnetic at low temperatures, it is thus possible to measure if the appearance of ferromagnetism leads to a SHE anisotropy.

The devices were patterned on PMMA, by conventional e-beam on a SiO2_2 substrate. The Cu, CoFe and Py wires were deposited by physical vapor deposition, while the NiCu was deposited by sputtering from a Ni60_{60}Cu40_{40} target followed by a lift-off, while Ni16_{16}Pd84_{84} was codeposited from a Ni and a Pd target. The CoFe electrodes were deposited in a first step, followed by the ISHE wire, and finally by the copper channel in a third step. We cleaned the interfaces in situ by Ion Beam Etching, prior to the deposition of the copper channel.

The magnetoresistance measurements have been performed using lock-in techniques (I=400 μAI = 400\,\mu\mathrm{A}, f=123f = 123 Hz). The non-local signal measured in a reference LSV without absorber (Figure 1b) is larger (Figure 1e) than the one detected in a device with a NiCu absorber (Figure 1d and 1f), with a signal amplitude going from 15 mΩ\Omega to 3.3 mΩ\Omega. This NL signal difference allows measuring the spin conductance of the absorbing SHE wire, and thus evaluating the amount of spin current absorbed by the ferromagnetic ISHE material [53].

In the device presented in Figure 2a, we performed both non-local measurements (cf. Figure 1c) and ISHE measurements (Figure 1d), with an ISHE signal amplitude of 120 μ\muΩ. Contrarily to what can be obtained using classical LSVs with FM materials [9], the signals can here be measured at low fields, allowing the control of the angle ϕ\phi in between the absorber magnetization and the spin current polarization (cf. Figure 2b). At low fields, the magnetization of the absorber is along YY, and thus transverse to the spin current polarization, which is along XX. At high fields, the magnetization of the absorber is along XX, and thus collinear to the spin current polarization.

Image not extracted

Figure 2. (a) colored SEM image of a LSV with a NiCu absorber. The central part of the device is additionally covered with a Cu thin film, to avoid spurious magnetoresistive contributions to the signal [53]. (b) Relative orientation between the spin current polarization σ\sigma and the magnetization of the absorber at low (ϕ=0\phi= 0) and high (ϕ=π/2\phi= \pi/2) fields. (c) NL signal at room temperature (red) and at 12 K (blue) using a 100 nm wide NiCu absorber. (d) two probe magnetoresistance of the 100 nm wide NiCu absorber measured at 12 K (blue) and at room temperature (red), for a magnetic field transverse to its easy magnetization axis. (f) ISHE measurement in a NiCu absorber, made simultaneously to the NL measurement shown in (c), and (e) scheme of the corresponding magnetic configurations.

Let us firstly focus on the non-local measurements. Us-

Using the measurement configuration of Figure 1c, clear non-local signals can be obtained for devices with NiCu absorbing wire, both in the ferromagnetic and the paramagnetic phase (cf. Figure 2c).

Adding the absorbing NiCu wire to the LSV leads to a strong decrease of the non-local signal (cf. Figure 1e vs. Figure 1f). The presence of the absorbing wire between the injecting and detecting CoFe electrode indeed leads to a partial absorption of the spin current flowing into the channel. The absorbed spin current is denoted jzxj_z^x, as it flows in the ZZ direction and has a spin polarization along XX. Its expression is given by the relation [26]:

jzx=Geff(m)μx(1)j_z^x = G_{\mathrm{eff}}(\mathbf{m})\mu^x \tag*{(1)}

with m^\hat{m} the magnetization direction of the absorber and μx\mu^x the spin accumulation along the xx direction at the interface between the Cu channel and the absorber. GeffG_{\mathrm{eff}} is treated as an effective parameter taking into account the spin conductance Gs=1/ρlsfG_s = 1/\rho l_{\mathrm{sf}} with ρ\rho and lsfl_{\mathrm{sf}} the resistivity and spin diffusion length of the absorbing material [41] (for m=x^\mathbf{m} = \hat{x}), or the spin mixing conductance G↑↓G_{\uparrow\downarrow} (m=y^\mathbf{m} = \hat{y} or z^\hat{z}) [41, 42], as well as the interface resistance RintR_{\mathrm{int}}.

We extracted from the NL signals GeffG_{\mathrm{eff}} and thus jzxj_z^x at the NiCu/Cu interface, using FEM simulations [8] (see [53] for computation details and extracted parameters). As seen in Figure 2c, the non-local signal at 12 K, and thus the absorbed spin current, is found to be relatively independent on the relative angle between the spin polarization and the absorber magnetization [53]. This absence of modulation, which contrasts with the results obtained in ref. [41] using Py, Co and CoFe as ferromagnetic absorbers, is possibly due to the relatively high interface resistance (7 fΩ⋅\Omega\cdot m2^2) between Cu and NiCu [53] when compared to the minimal Sharvin interfacial resistance at the copper 3d-FM interface (0.8 fΩ⋅\Omega\cdot m2^2) [41]. The modulation being smaller than the experimental error bar, the values of the spin conductance and of the effective spin mixing conductance can be considered to be equal.

Now that the absorbed spin current is known, let us focus on the ISHE. We firstly measured the dependence of the magnetization direction of the NiCu SHE absorber as a function of the field applied along X, by performing two probe magnetoresistance measurements of the NiCu wire (Figure 2d). The magnon magnetoresistance contribution [43, 44] dominates the signal in both the paramagnetic and ferromagnetic phases. In the ferromagnetic phase, the magnetoresistance also displays at low fields a deviation from the linear behavior, corresponding to the expected anisotropic magnetoresistance. This allows measuring the saturation field of the NiCu wire (Bc=0.2B_c = 0.2 T) along the X axis (ϕ=π/2\phi= \pi/2).

We then measured the ISHE signal using the configuration of Figure 1d, at both 12 K and 300 K. The Curie temperature of Ni60_{60}Cu40_{40} has been found to be around 220 K for this composition [28]. Using the non-local and ISHE measurements, we extracted an effective spin Hall angle (2.3%) consistent with the one of ref. [28] measured using spin pumping, which confirms the validity of our measurement method [53]. The ISHE signal, shown in Figure 2f, is a square loop in both the paramagnetic and ferromagnetic phases. The observed square loops reflect the change of sign of the absorbed spin current polarization when reversing the injector magnetization. The symmetry and shape of the signal correspond to what can be expected from the ISHE symmetries, and from the switching fields measured in the non-local configuration. The parallel and transverse ISHE signals can be obtained as ΔRISHE⊥=RB−RE\Delta R_{\mathrm{ISHE}}^{\perp} = R^B - R^E and ΔRISHE∥=RA−RD\Delta R_{\mathrm{ISHE}}^{\parallel} = R^A - R^D, RiR^i being the electric potential drop in the magnetic state ii reported in Figure 2e. The key finding is that at 12 K, the ISHE signal is constant in the [−0.2 T; 0.2 T][-0.2\ \mathrm{T};\ 0.2\ \mathrm{T}] field range, where the magnetization of the absorber rotates from the XX to the YY direction, so that ΔRISHE⊥=ΔRISHE∥\Delta R_{\mathrm{ISHE}}^{\perp} = \Delta R_{\mathrm{ISHE}}^{\parallel}. This means that the ISHE is independent on the direction of the absorber magnetization. This isotropy of the ISHE in the ferromagnetic phase is also illustrated by the fact that very similar loops in shape are observed in the paramagnetic phase, where one does not expect any anisotropy, and in control devices using Pt as absorber [53].

We also performed similar measurements using a 15 nm thick Ni16_{16}Pd84_{84} ferromagnetic absorber, in which the origin of the ISHE is extrinsic [45] while it is intrinsic in NiCu [28]. This alloy is ferromagnetic below 230 K. It has an out of plane magnetization at low temperature [53], but in-plane above 150 K (cf. Figure 3c). In order to avoid the strain induced magnetic inhomogeneity associated with an out of plane magnetization in this material [46], we measured the ISHE and non-local signal at 150 K when NiPd is still magnetic, and its magnetization is in plane. Similarly to the case of NiCu, the ISHE signal is found to be isotropic with respect to the magnetization direction.

Image not extracted

Figure 3. ((a) Non-local and (b) ISHE (d) signals measured during the same magnetic field sweep, at 150 K with a 100 nm NiPd absorber.

The ISHE thus appears to be isotropic both for NiCu and NiPd in their ferromagnetic phase. This result is very surprising, as there is a symmetry breaking induced by the appearance of the magnetization at the paramagnetic/ferromagnetic transition. Theoretical studies have indeed predicted a sizeable modulation of the interconversion when rotating the magnetization [15, 47].

Let us now look at the links between this isotropy of the signal and the spin transport parameters. The absorbed spin current JcJ_{\mathrm{c}} is converted into a charge current JsJ_{\mathrm{s}} according to Jc=θJsJ_{\mathrm{c}} = \theta J_{\mathrm{s}}. Importantly, θ\theta is not the sole figure of merit of the ISHE. The conversion indeed occurs only over a limited material thickness, roughly equal to the spin relaxation length, after which the spin current, which is not conserved, vanishes. The produced signal is thus actually proportional to the product of the spin Hall angle by the spin relaxation length. If the incoming spins are collinear to the magnetization, this product is θ∥lsf\theta_{\parallel}l_{\mathrm{sf}}, where θ∥\theta_{\parallel} is the spin Hall angle in the collinear situation. If the incoming spins are transverse to the magnetization, this product becomes θ⊥\theta_{\perp} times λ⊥\lambda_{\perp}, with λ⊥\lambda_{\perp} the transverse spin relaxation length. λ⊥\lambda_{\perp} represents the ballistic relaxation by phase averaging of the spin current with a polarization transverse to the magnetization. The isotropy of the ISHE signal suggests that in our experiments:

θ∥lsf∼θ⊥λ⊥(2)\theta_{\parallel}l_{\mathrm{sf}} \sim\theta_{\perp}\lambda_{\perp} \tag*{(2)}

In principle, it is possible to measure separately lsfl_{\mathrm{sf}} and λ⊥\lambda_{\perp}, as they affect the spin absorption [41]. lsfl_{\mathrm{sf}} has been measured in NiCu [28] and is equal to 2.4 nm at room temperature. The measurement of λ⊥\lambda_{\perp} is more complex. The presence of a large interface resistance prevents here the observation of the spin absorption anisotropy in our devices. It also has the effect of keeping the amount of spin current contributing to the ISHE constant. Extracting λ⊥\lambda_{\perp} would require thickness dependence measurement [32] with all the spurious effects linked film thickness reduction [48].

An estimation of λ⊥\lambda_{\perp} can be obtained by assuming that it is inversely proportional to the exchange field [49], and thus to the Curie temperature [50]. By taking as reference material Py, which has a TcT_{\mathrm{c}} of 800 K [51] and an exchange constant of JPy∼100J_{\mathrm{Py}} \sim100 meV with λ⊥Py∼1\lambda_{\perp}^{\mathrm{Py}} \sim1 nm [41, 49], λ⊥\lambda_{\perp} in NiCu can be estimated to be λ⊥NiCu∼5\lambda_{\perp}^{\mathrm{NiCu}} \sim5 nm with JNiCu∼20J_{\mathrm{NiCu}} \sim20 meV. The transverse relaxation length due to ballistic effects in NiCu is therefore larger than its spin diffusion length. This means that the transverse spin current relaxes mainly over the spin diffusion length through diffusive processes and that λ⊥NiCu=lsf\lambda_{\perp}^{\mathrm{NiCu}} = l_{\mathrm{sf}}. θ∥\theta_{\parallel} has been estimated to be 2.3% [53], which would lead according to our experimental result of eq. (2) to the same value for θ⊥\theta_{\perp}. The case of NiPd is more difficult to analyse since we do not have values of the spin diffusion length in this material. However, the combination of the large SO interaction evidenced by the out of plane magnetic anisotropy at low temperature, and small exchange interaction evidenced by the low Curie temperature makes us expect a similar relation between the transverse spin relaxation and the spin diffusion lengths.

In light of these results, it appears that the isotropy of the absorption is to be expected in low-TcT_{\mathrm{c}} FMs with strong spin-orbit coupling since the low exchange interaction drives the transverse spin relaxation length to be equal to the spin diffusion length. Hence, from the eq. (2) we can conclude that the spin Hall angle in NiCu and NiPd is isotropic. The picture in high-TcT_{\mathrm{c}} FMs is however more contrasted. Indeed, it has been established that a strong anisotropy of the absorption exists in these materials [41]. The isotropy of the ISHE signal has been observed in CoFe [17] and Py [16], where the relation given by eq. (2) does not seem to hold [32], while it does in Co [31]. According to theoretical studies [15], the details of the SOC effect on the band structure of these materials would provide the explanation for these behaviors, and we believe that the device described in this paper can provide an important tool for a systematic investigation of these phenomena.

To conclude, we proposed a device allowing the measurement of the anisotropy of the spin-charge interconversion in ferromagnetic materials. Although the paramagnetic/ferromagnetic transition is associated to symmetry breaking, the ISHE signal in NiCu and NiPd remains surprisingly independent of the magnetization direction in the ferromagnetic phase. In terms of spin transport properties, this implies that the product of the SHA by the spin relaxation length is the same in the colinear and transverse configuration. In the studied low TcT_{\mathrm{c}} materials, this can be understood by the long transverse relaxation length which causes the spin current to relax during scattering on SO impurities and therefore to be equal to the spin diffusion length. The isotropy of the spin Hall angle is however not explained by these considerations and will require a more systematic theoretical and experimental work.

We acknowledge the financial support by ANR French National Research Agency OISO (ANR-17-CE24-0026). This project also received funding from the EUropen Union’s Horizon 2020 research and innovation program under the Marie Slodowska-Curie Grant Agreement No. 955671.

The data associated to the figures can be found at the following link https://doi.org/10.57745/Z3BG2U.

References

References

  1. [1]T. Valet and A. Fert, "Theory of the perpendicular magnetoresistance in magnetic multilayers ", Phys. Rev. B 48, 7099 (1993).pubmed.ncbi.nlm.nih.gov/10006879
  2. [2]M. D. Stiles and A. Zangwill, "Anatomy of spin-transfer torque", Phys. Rev. B 66, 014407 (2002).DOI
  3. [3]Q. Shao et al, "Roadmap of spin-orbit torques", IEEE Transactions on Magnetics (2021).DOI
  4. [4]S. Manipatruni et al, "Scalable energy-efficient magnetoelectric spin-orbit logic" Nature, 565(7737), 35 (2019).DOI
  5. [5]J. Sinova, S. O. Valenzuela, J. Wunderlich, C.H. Back, and T. Jungwirth, "Spin Hall effects" Rev. Mod. Phys. 87, 1213 (2015).
  6. [6]Y. K. Kator, C. Myersa. C. Gossardand, D. D. Awschalom, "Observation of the Spin Hall Effect in Semiconductors", Science 306, 1910 (2004).pubmed.ncbi.nlm.nih.gov/15539563
  7. [7]Y. Tserkovnyak, A. Brataas, and G. E. W. Bauer, "Spin pumping and magnetization dynamics in metallic multi- layers" Phys. Rev. B 66, 224403 (2002).DOI
  8. [8]P. Laczowski, M. Cosset-Cheneau, W. Savero-Torres, V. T. Pham, G. Zahnd, H. Jaffres, N. Reyren, J.-C. Rojas-Sanchez, A. Marty, L. Vila, J.-M. George, and J.-P. Attane, "Spin-dependent transport characterization in metallic lateral spin valves using one-dimensional and three-dimensional modeling", Phys. Rev. B 99, 134436 (2019).DOI
  9. [9]Y. Omori, E. Sagasta, Y. Niimi, M. Gradhhand, L. E. Hueso, F. Casanova, and Y. Otani, "Relation between spin Hall effect and anomalous Hall effect in 3d ferromagnetic metals", Phys. Rev. B 99, 014403 (2019).DOI
  10. [10]S. Wimmer, H. Ebert, S. Gambarelli, M. Chshiev, and V. Baltz, "Self-induced inverse spin Hall effect in ferromagnets: Demonstration through nonmonotonic temperature dependence in permalloy" Phys. Rev. B 100, 174409 (2019).DOI
  11. [11]T. Taniguchi, J. Grollier and M.D. Stiles "Spin-Transfer Torque Generated by the Anomalous Hall Effect in Anisotropic Magnetoresistance" Phys. Rev. Applied 3, 044001 (2015).
  12. [12]M. Kimata, H. Chen, K. Kondou, S. Sugimoto, P. K. Muduli, M. Ikhlas, Y. Omori, T. Tomita, A. H. MacDonald, S. Nakatsuji and Y. Otani, "Magnetic and magnetic inverse spin Hall effects in a non-collinear antiferromagnet", Nature 565, 627-630 (2019).DOI
  13. [13]Y. Hibino, T. Taniguchi, K. Yakushiji, A. Fukushima, H. Kubota and S. Yuasa, "Giant charge-to-spin conversion in ferromagnet via spin-orbit coupling", Nat Commun 12, 6254 (2021).DOI
  14. [14]Angie Davidson, Vivek P.Amin, Wafa S.Aljuaid, Paul M.Haney, Xin Fan, "Perspectives of electrically generated spin currents in ferromagnetic materials", Phys. Lett. A 384, 126228 (2020).DOI
  15. [15]V. P. Amin, Junwen Li, M. D. Stiles, and P. M. Haney, "Intrinsic spin currents in ferromagnets", Phys. Rev. B 99, 220405(R) (2019).DOI
  16. [16]K. S. Das, W.Y. Schoemaker, B.J. van Wees, and I.J.Vera-Marun, "Spin injection and detection via the anomalous spin Hall effect of a ferromagnetic metal", Phys. Rev. B 96, 220408(R) (2017).DOI
  17. [17]T. Wimmer, B. Coester, S. Geprag, R. Gross, S.T.B. Goennenwein, H. Huebl, and M. Althammer, "Anomalous spin Hall angle of metallic ferromagnet determined by a multimaterial spin injection/detection device" Appl. Phys. 115, 092404 (2019).DOI
  18. [18]D. Tian, Y. Li, D. Qu, S. Y. Huang, X. Jin, and C. L. Chien, "Manipulation of pure spin current in ferromagnetic metals independent of magnetization", Phys. Rev. B 94, 020403(R) (2016).DOI
  19. [19]K. Ando, S. Takahashi, J. Ieda, Y. Kajiwara, H. Nakayama, T. Yoshino, K. Harii, Y. Fujikawa, M. Matsuo, S. Maekawa, and E. Saitoh, "Inverse spin-Hall effect induced by spin pumping in metallic system", J. Appl. Phys. 109, 103913 (2011).DOI
  20. [20]V.T. Pham, L. Vila, G. Zahnd, A. Marty, W. Savero-Torres, M. Jamet and J.P. Attane, "Ferromagnetic/nonmagnetic nanostructures for the electrical measurement of the spin Hall effect", Nano Lett. 16, 11, 6755 (2016).pubmed.ncbi.nlm.nih.gov/27712075
  21. [21]S. O. Valenzuela and M. Tinkham "Direct electronic measurement of the spin Hall effect", Nature 442, 176 (2006).DOI
  22. [22]J. Kim, P. Sheng, S. Takahashi, S. Mitani, and M. Hayashi "Spin Hall Magnetoresistance in Metallic Bilayers", Phys. Rev. Lett. 116, 097201 (2016).DOI
  23. [23]K. Uchida, S. Takahashi, K. Harii, J. Ieda, W. Koshibae, K. Ando, S. Maekawa and E. Saitoh, "Observation of the spin Seebeck effect", Nature 455, 778 (2008).DOI
  24. [24]L. Liu, T. Moriyama, D. C. Ralph, and R. A. Buhrman "Spin-Torque Ferromagnetic Resonance Induced by the Spin Hall Effect" Phys. Rev. Lett. 106, 036601 (2011).DOI
  25. [25]M. Hayashi, J. Kim, M. Yamanouchi, and H. Ohno "Quantitative characterization of the spin-orbit torque using harmonic Hall voltage measurements", Phys. Rev. B 89, 144425 (2014).DOI
  26. [26]Y.-T. Chen, S. Takahashi, H. Nakayama, M. Althammer, S.T.B. Goennenwein, E. Saitoh, and G.E.W. Bauer, "Theory of spin Hall magnetoresistance", Phys. Rev. B 87, 144411 (2013).DOI
  27. [27]J. Cramer, A. Ross, S. Jaiswal, L. Baldrati, R. Lebrun, and M. Kläui "Orientation-dependent direct and inverse spin Hall effects in Co60Fe20B20" Phys. Rev. B 99, 104414 (2019).
  28. [28]S. Varotto, M. Cosset-Cheneau, C. Grezes, Y. Fu, P. Warin, A. Brenac, J.-F. Jacquot, S. Gambarelli, C. Rinaldi, V. Baltz, J.-P. Attane, L. Vila, and P. Noel, "Independence of the Inverse Spin Hall Effect with the Magnetic Phase in Thin NiCu Films", Phys. Rev. Lett. 125, 267204 (2020).DOI
  29. [29]Y. Ou, Z. Wang, C.S. Chang, H. P. Nair, H. Paik, N. Reynolds, D. C. Ralph, D. A. Muller, D. G. Schlom, and R. A. Buhrman, "Exceptionally High, Strongly Temperature Dependent, Spin Hall Conductivity of SrRuO3", Nano Lett., 19, 6, 3663 (2019).DOI
  30. [30]J. D. Gibbons, D. MacNeill, R. A. Buhrman, and D. C. Ralph, "Reorientable Spin Direction for Spin Current Produced by the Anomalous Hall Effect" Phys. Rev. Applied 9, 064033 (2018).DOI
  31. [31]B. F. Miao, S.Y. Huang D. Qu and C. L. Chien, "Inverse Spin Hall Effect in a Ferromagnetic Metal", Phys. Rev Lett. 111, 066602 (2013).pubmed.ncbi.nlm.nih.gov/23971597
  32. [32]Z. Zhu, X. Zheng, G. Li, H. Bai, J. Su, Y. Zhang and J.-W. Cai, "Strong spin orientation-dependent spin current diffusion and inverse spin Hall effect in a ferromagnetic metal", NPG Asia Mater 12, 12 (2020).DOI
  33. [33]H. Mizuno, H. Isshiki, K. Kondou, Y. Zhu, and Y. Otani, "Influence of planar Hall effect on the output signal in a T-shaped spin conversion device", Appl. Phys. Lett. 119, 092401 (2021).DOI
  34. [34]I. Groen, V.T. Pham, N. Leo, A. Marty, L. E. Hueso, and F. Casanova, "Disentangling Spin, Anomalous, and Planar Hall Effects in Ferromagnet-Heavy-Metal Nanostructures", Phys. Rev. Applied 15, 044010 (2021).DOI
  35. [35]G. Zahnd, L. Vila, V. T. Pham, M. Cosset-Cheneau, W. Lim, A. Brenac, P. Laczkowski, A. Marty, and J. P. Attane, "Spin diffusion length and polarization of ferromagnetic metals measured by the spin-absorption technique in lateral spin valves", Phys. Rev. B 98, 174414 (2018).DOI
  36. [36]Y. Niimi, Y. Otani, "Reciprocal spin Hall effects in conductors with strong spin-orbit coupling: a review" Rep. Prog. Phys. 78 124501 (2015).DOI
  37. [37]J.-C. Rojas Sanchez, P. Laczkowski, W. F. Savero Torres, M. Cubukcu, V. D. Nguyen, L. Notin, C. Beigne, C. Vergnaud, A. Marty, M. J. May, L. Vila, and J. P. Attané, "In-plane and out-of-plane spin precession in lateral spin-valves", Appl. Phys. Lett. 102, 132408 (2013).DOI
  38. [38]G. Zahnd, L. Vila, V. T. Pham, F. Roclais, M. Cosset-Cheneau, C. Vergnaud, M. Jamet, P. Noel, T. Gushi, A. Brenac, A. Marty, and J. P. Attané, "Observation of the Hanle effect in giant magnetoresistance measurements", Appl. Phys. Lett. 112, 232405 (2018).DOI
  39. [39]G. Zahnd, L. Vila1, T.V. Pham, A. Marty, P. Laczkowski, W. Savero Torres, C. Beigné, C. Vergnaud, M. Jamet and J.-P. Attané, "Comparison of the use of NiFe and CoFe as electrodes for metallic lateral spin valves", Nanotechnology 27 035201 (2016).DOI
  40. [40]L. Vila, T. Kimura and Y. Otani, "Evolution of the Spin Hall Effect in Pt Nanowires: Size and Temperature Effects", Phys. Rev. Lett. 99, 266604 (2007).DOI
  41. [41]M. Cosset-Chéneau, L. Vila, G. Zahnd, D. Gusakova, V.T. Pham, C. Grezes, X. Waintal, A. Marty, H. Jaffres, and J.-P. Attané, "Measurement of the Spin Absorption Anisotropy in Lateral Spin Valves", Phys. Rev. Lett. 126, 027201 (2021).DOI
  42. [42]A. Brataas, G.E.W.Bauer, P. J.Kelly, "Non-collinear magnetoelectronics", Phys. Rep. 427, 157 (2006).DOI
  43. [43]A. P. Mihai, J. P. Attané, A. Marty, P. Warin, and Y. Samson, "Electron-magnon diffusion and magnetization reversal detection in FePt thin films", Phys. Rev. B 77, 06401(R) (2008).DOI
  44. [44]V. D. Nguyen, L. Vila, P. Laczkowski, A. Marty, T. Faivre, and J. P. Attané, "Detection of domain-wall position and magnetization reversal in nanostructures using the magnon contribution to the resistivity", Phys. Rev. Lett. 107, 136605 (2011).pubmed.ncbi.nlm.nih.gov/22026884
  45. [45]D.H. Wei, Y. Niimi, B. Gu, T. Ziman, S. Maekawa and Y. Otani, "The spin Hall effect as a probe of nonlinear spin fluctuations", Nat Commun 3, 1058 (2012).DOI
  46. [46]H. Z. Arham, Trupti S. Khaire, R. Loloee, W. P. Pratt, Jr., and Norman O. Birge, "Measurement of spin memory lengths in PdNi and PdFe ferromagnetic alloys", Phys. Rev. B 80, 174515 (2009).DOI
  47. [47]G. Qu, N. K. Nakamura, and M. Hayashi, "Magnetization direction dependent spin Hall effect in 3d ferromagnets", Phys. Rev. B 102, 144440 (2020).DOI
  48. [48]C. Gonzalez-Fuentes, C. Henriquez, C. Garcia, R. K. Dumas, B. Bozzo, and A. Pomar, "Spin diffusion length associated with out-of-plane conductivity of Pt in spin pumping experiments" Phys. Rev. B 103, 224403 (2021).DOI
  49. [49]C. Petitjean, D. Luc, and X. Waintal, "Unified Drift-Diffusion Theory for Transverse Spin Currents in Spin Valves, Domain Walls, and Other Textured Magnets" Phys. Rev. Lett. 109, 117204 (2012).pubmed.ncbi.nlm.nih.gov/23005670
  50. [50]I. Turek, J. Kudrnovsky, V. Drchal and P. Bruno "Exchange interactions, spin waves, and transition temperatures in itinerant magnets" Philos. Mag. 86:12, 1713-1752 (2006).
  51. [51]X. Zhang, Y. Lao, J. Sklenar, N. S. Bingham, J. T. Batley, J. D. Watts, C. Nisoli, C. Leighton, and P. Schiffer, "Understanding thermal annealing of artificial spin ice", APL Materials 7, 111112 (2019).DOI
  52. [52]M.W. Keller, K.S. Gerace, M. Arora, E. K. Delczeg-Czirjak, J. M. Shaw, and T. J. Silval, "Near-unity spin Hall ratio in NiCu alloys" Phys. Rev. B 99, 214411 (2019).
  53. [53]See Supplemental Material.

Paper details

vlnc:W_yzb6j26e
Version
v1 · latest
Published
Fresh — added to the Hub within the last 30 days
Added
License
CC BY 4.0
Usage

views · 0

downloads · 0

A view counts once per browser per day, a download each time the PDF is requested.

  • Physics and Astronomy

Not recorded for this paper

View statement
Looking for related papers…
Contents