betaFeedback

WorksPhysics and Astronomy

DFT based investigation of the structural, magnetic, electronic, and half-metallic properties of solid In1−x_{1-x}Tix_{x}Sb solutions

Abstract

With the intention to reveal the effect of the substitution, Ti-doped InSb alloy, we accomplished a first-principles prediction within the FPLAPW+lo method. We used GGA-PBEsol scheme attached with the improved TB-mBJ approach to predict structural, electronic, and magnetic properties of In1−x_{1-x}Tix_{x}Sb with concentration x=0x = 0, 0.1250.125, 0.250.25, 0.500.50, 0.750.75, 0.8750.875, and 11. Our lattice parameters are found in favorable agreement with the available theoretical and experimental data. The calculation shows that all structures are energetically stable. The substitutional doping transforms the ionic character of the InSb compound in half-metallic ferromagnetic comportment for concentration x=0x = 0, 0.1250.125, 0.250.25, and 0.500.50, with a spin polarization of 100100% at the Fermi level, and metallic nature for In0.25_{0.25}Ti0.75_{0.75}Sb and In0.125_{0.125}Ti0.875_{0.875}Sb. The total magnetic moments are also estimated at about 1 μBμ_{\text{B}}. In0.875_{0.875}Ti0.125_{0.125}Sb, In0.75_{0.75}Ti0.25_{0.25}Sb, and In0.50_{0.50}Ti0.50_{0.50}Sb have half-metallic ferromagnets comportment and they can be upcoming applicants for spintronics applications.

Introduction

The possibility to dope the semiconductors with magnetic elements has created a new category of materials called diluted magnetic semiconductors (DMS). One of the peculiarities of DMS is the appearance of localized magnetic moments generated by electron-hole coupling [1]. This leads to interesting properties, for example, increasing the gg factor of the charge carriers or new excitements, such as magnetic polarons [2]. However, ferromagnetism is rarely observed in semiconductors due to the low density of carriers and because of the predominance of superexchange between local magnetic moments. In most cases, magnetic semiconductors have low Curie temperatures. Interest in DMSs was recently aroused by theoretical and experimental work on semiconductors [3, 4, 5, 6, 7, 8, 9, 10, 11, 12, 13, 14, 15, 16, 17, 18, 19]. DMS based on the transition element doped and on semiconductors has two important characteristics. The first one, the transition concentration of the elements can be up to ten percent (using molecular beam epitaxy techniques, MBE) [20]. The second one, the concentration of carriers can be controlled in a wide range and permits to choose between nn-type and pp-type doping. These two aspects offer the possibility of varying the magnetic behavior by changing the concentration of the carriers. Indium Antimonide is one of the best frequently exploited semiconductors, which is used in Hall effect sensors, thermoelectric generators, infrared detectors, high-speed photodetectors, and transistors [21, 22, 23, 24, 25, 26, 27, 28, 29, 30, 31]. This extensive utilization follows from its distinct properties, such as a narrow band gap, small effective electron mass, and high electron mobility. Doping different materials into the InSb structure fascinates several scientists. Consequently, the category of dopant strongly influences InSb characteristics and should be precisely chosen according to suitable properties

This work is licensed under a Creative Commons Attribution 4.0 International License. Further distribution of this work must maintain attribution to the author(s) and the published article’s title, journal citation, and DOI. and future applications. The optimization of pulse electrodeposition method for the synthesis of Te-doped InSb films was performed by Rajská et al. [32]. They show that the bandgap values affirm an impact of a dopant content on the optical properties of thin Te-doped InSb films. The maximum figure of merit (ZT) was found to be about 0.6 and 673 K for Te-doped InSb [33]. They conclude that this material is a very promising candidate for thermoelectric devices. The transport properties of Sn-doped InSb, were experimentally studied by Okamoto and Shibasaki [34] and confirm its use in Hall sensors applications. InSb doped with magnetic elements for spintronics applications has been the patience of several researchers. Theoretical and experimental studies have been carried out to describe the magnetic phenomenon and the half-metallicity comportment. Mn-doped InSb was studied by Novotortsev et al. [35], (Fe, Mn, and Cr) doped InSb [36, 37, 38, 39, 40, 41, 42, 43]. The aim of our study is to predict structural, electronic, and magnetic properties of Ti-doped InSb.

Computational method

With the intention of calculating appropriate properties of Ti-doped InSb, we performed calculations within the full-potential linearized augmented plane wave (FP-LAPW) method [44, 45, 46, 47] based on the density functional theory (DFT) [47, 48] implemented in WIEN2k code [48]. We employed Perdew–Burke–Ernzerhof GGA-PBEsol approximation [49], combined with Tran–Blaha modified Becke–Johnson TB-mBJ approximation [50, 51, 52].In our calculation, we used the following parameters:

  • KmeshK_{\mathrm{mesh}} 200 k-points in Brillion zone (BZ).

  • The muffin-tin radii for Ti, In, and Sb are chosen as 1.65, 1.85, and 1.96 a.u., respectively.

  • RMT⋅Kmax=7R_{\mathrm{MT}} \cdot K_{\mathrm{max}} = 7, where RMTR_{\mathrm{MT}} is the smallest value of muffin-tin sphere radius, and KmaxK_{\mathrm{max}} indicates the largest vector in-plane wave expansion.

  • lmax=6l_{\mathrm{max}} = 6, where lmaxl_{\mathrm{max}} is the wave function inside the muffin-tin spheres.

  • Gmax=14G_{\mathrm{max}} = 14, where GmaxG_{\mathrm{max}} is the magnitude largest vector in the charge density Fourier expansion.

  • The cut-off energy selected as −6 Ry (the separation of valence and core states ).

  • The self-consistent calculations are converged when the condition is set to 0.0001 Ry.

  • Employing configuration 2×2×22 \times2 \times2, a supercell of In8_8Sb8_8 with (Zincblende, F4 3m, space group N:216) was constructed, which, consists of 16 atoms in which 8 atoms belong to Indium and 8 atoms belong to Antimonide. The doping of Titanium cation was done on an In1−x_{1-x}Tix_xSb structure. In0.875_{0.875}Ti0.125_{0.125}Sb, In0.75_{0.75}Ti0.25_{0.25}Sb, In0.50_{0.50}Ti0.50_{0.50}Sb, In0.25_{0.25}Ti0.75_{0.75}Sb, and In0.125_{0.125}Ti0.875_{0.875}Sb structures were

created by Ti atom on substitution sites with Indium. The relaxation maintained the F4 3m symmetry for the structure investigated.

Results and discussion

Structural properties

Indium Antimonide (InSb) crystallizes in the zincblende structure (No. 216). Figure 1 exhibits the crystal supercell structure of InSb. Its conventional structure has two types of atoms, In and Sb, located at (0, 0, 0) and (0.25, 0.25, 0.25) positions, respectively [56, 57]. The In0.875_{0.875}Ti0.125_{0.125}Sb, In0.75_{0.75}Ti0.25_{0.25}Sb, In0.50_{0.50}Ti0.50_{0.50}Sb, In0.25_{0.25}Ti0.75_{0.75}Sb, and In0.125_{0.125}Ti0.875_{0.875}Sb compounds are constructed by substitutional doping of one (1/8 = 0.125), two (2/8 = 0.25), four (4/8 = 0.50), six (6/8 = 0.75) and seven (7/8 = 0.875) atoms of Titanium (Ti) at Indium (In) sites, respectively. The structures of In1−x_{1-x}Tix_xSb with concentration x=0x = 0 (InSb), 0.125, 0.25, 0.50, 0.75, 0.875, and 1 (TiSb) are completely optimized and relaxed. For both ferromagnetic (FM) and non-ferromagnetic (NFM) phases, the energy curves as a function of the volume of each structure (see Figure 2) are calculated and fitted by the suitableness of Birch–Murnaghan’s equation of state (EOS) [58]. According to Figure 2, all the structures are stable in the FM phase except the binary InSb. In this respect, we estimated the structural properties including the equilibrium lattice constant “aa”, bulk modulus “B0B_0”, and its derivative B′B^{\prime}. The results are collected in Table 1 accompanied by the available theoretical and experimental data. The thermodynamic stability and the probability of synthesizing these alloys [59, 60] are determined by the formation and cohesive energies. To confirm the phase stability of the In0.875_{0.875}Ti0.125_{0.125}Sb, In0.75_{0.75}Ti0.25_{0.25}Sb, In0.50_{0.50}Ti0.50_{0.50}Sb, In0.25_{0.25}Ti0.75_{0.75}Sb, and In0.125_{0.125}Ti0.875_{0.875}Sb structures, we calculated the formation and cohesive energies using the following expressions [43, 44]:

Image not extracted

Figure 1. (Colour online) Crystal supercell structure of InSb.

Compoundaa (Å)BB (GPa)B′B'EFormE_{\mathrm{Form}}EcohE_{\mathrm{coh}}Method
This WorkGGA-WC
InSb6.555442.46124.0525
In0.875_{0.875}Ti0.125_{0.125}Sb6.4876, 6.5069 [53]39.79535.0000−0.3410.941
In0.75_{0.75}Ti0.25_{0.25}Sb6.4455, 6.4585 [53]54.20425.0000−0.5220.852
In0.50_{0.50}Ti0.50_{0.50}Sb6.3878, 6.3616 [53]52.03056.7370−0.4350.902
In0.25_{0.25}Ti0.75_{0.75}Sb6.3087, 6.2648 [53]53.84142.9134−0.4760.871
In0.125_{0.125}Ti0.875_{0.875}Sb6.2315, 6.2164 [53]62.18054.7886−0.3930.932
TiSb6.169758.07554.3008
Other calculations
InSb6.464, 6.36 [28]
6.479 [29]
6.643 [30]
6.629 [31]37.368 [31]4.452 [31]GGA-PBE
6.47937 [32], 6.4791 [54]Experimental
6.49 [34], 6.47937 [55]Experimental

Table 1. Calculated lattice constant (aa), bulk modulus (BB), and its pressure derivative (B′B') for for In1−x_{1-x}Tix_xSb at concentrations x=0x = 0, 0.125, 0.25, 0.50, 0.75, 0.875 and 1.

Image not extracted

Figure 2. (Colour online) Energy unit cell versus volume with FM and NFM phase of (a) InSb, (b) In0.875_{0.875}Ti0.125_{0.125}Sb, (c) In0.75_{0.75}Ti0.25_{0.25}Sb, (d) In0.50_{0.50}Ti0.50_{0.50}Sb, (e) In0.25_{0.25}Ti0.75_{0.75}Sb, (f) In0.125_{0.125}Ti0.875_{0.875}Sb, and (g) TiSb.

EformIn1−xTixSb=EtotalIn1−xTixSb−[(1−x)EsolidIn+xEsolidTi+8EsolidSb](1)E_{\mathrm{form}}^{\mathrm{In}_{1-x}\mathrm{Ti}_x\mathrm{Sb}} = E_{\mathrm{total}}^{\mathrm{In}_{1-x}\mathrm{Ti}_x\mathrm{Sb}} - \left[(1-x)E_{\mathrm{solid}}^{\mathrm{In}} + xE_{\mathrm{solid}}^{\mathrm{Ti}} + 8E_{\mathrm{solid}}^{\mathrm{Sb}}\right] \tag*{(1)}
EcohIn1−xTixSb=[(1−x)EatomIn+xEatomTi+8EatomSb]−EtotalIn1−xTixSb(2)E_{\mathrm{coh}}^{\mathrm{In}_{1-x}\mathrm{Ti}_x\mathrm{Sb}} = \left[(1-x)E_{\mathrm{atom}}^{\mathrm{In}} + xE_{\mathrm{atom}}^{\mathrm{Ti}} + 8E_{\mathrm{atom}}^{\mathrm{Sb}}\right] - E_{\mathrm{total}}^{\mathrm{In}_{1-x}\mathrm{Ti}_x\mathrm{Sb}} \tag*{(2)}

Here EtotalIn1−xTixSbE_{\mathrm{total}}^{\mathrm{In}_{1-x}\mathrm{Ti}_x\mathrm{Sb}} is the total energy per atom of In1−x_{1-x}Tix_xSb and EsolidInE_{\mathrm{solid}}^{\mathrm{In}}, EsolidTiE_{\mathrm{solid}}^{\mathrm{Ti}}, and EsolidSbE_{\mathrm{solid}}^{\mathrm{Sb}} are the total energies per atom of In, Ti, and Sb solids, respectively. EatomInE_{\mathrm{atom}}^{\mathrm{In}}, EatomTiE_{\mathrm{atom}}^{\mathrm{Ti}}, and EatomSbE_{\mathrm{atom}}^{\mathrm{Sb}} are the isolated atomic energies of the pure constituents of In, Ti, and Sb, respectively. Our computed values of formation and cohesive energies for In0.875_{0.875}Ti0.125_{0.125}Sb, In0.75_{0.75}Ti0.25_{0.25}Sb, In0.50_{0.50}Ti0.50_{0.50}Sb, In0.25_{0.25}Ti0.75_{0.75}Sb, and In0.125_{0.125}Ti0.875_{0.875}Sb compounds are collected in table 1. Therefore, the negative values of the formation energy and the positive values of cohesive energy, imply that the ternary alloys In1−x_{1-x}Tix_xSb with concentration x=0x = 0 (InSb), 0.125, 0.25, 0.50, 0.75, 0.875, and 1 (TiSb) are energetically and thermodynamically stable and can be synthesized under normal conditions. The deviation of a lattice constant aa as a function of the composition (xx) for In1−x_{1-x}Tix_xSb is shown in Figure 3. The linear relationship between the lattice constant and the dopant concentration xx [53] is predicted by Vegard’s law as follows:

Image not extracted

Figure 3. (Colour online) The calculated lattice constant aa of In1−x_{1-x}Tix_xSb as a function of concentration (xx).

a(x)=6.5554−0.3875x.(3)a(x) = 6.5554 - 0.3875x. \tag*{(3)}

However, the quadratic relationship is widely used for both experimental and theoretical purposes. We obtained the fitting equation for In1−xTixSb\mathrm{In}_{1-x}\mathrm{Ti}_{x}\mathrm{Sb}:

a(x)=6.53614−0.26049x−0.09602x2.(4)a(x) = 6.53614 - 0.26049x - 0.09602x^{2}. \tag*{(4)}

Electronic properties

In this section, we calculated the electronic properties result in the band structure, total and partial densities of state schemes. The calculations were performed for In1−xTixSb\mathrm{In}_{1-x}\mathrm{Ti}_{x}\mathrm{Sb} with different composition xx (x=0,0.125,0.25,0.50,0.75,0.875x = 0, 0.125, 0.25, 0.50, 0.75, 0.875 and 11), employing GGA-PBEsol associated with TB-mBJ of Tran–Blaha modified Becke–Johnson approximation [50, 51, 52, 61]. Figure 4 (a) and Figure 4 (b) exhibit the spin-polarized band structure of the binary InSb (x=0x = 0), and display that the two spin channels of

Image not extracted

Figure 4. (Colour online) Spin-polarized band structure obtained with TB-mBJ for InSb: (a) majority spin (up) and (b) minority spin (dn). The Fermi level is set to zero (horizontal dotted red line).

InSb have identical semiconducting band structures with a direct bandgap located between and high-symmetry points. The band structures of In0.875_{0.875}Ti0.125_{0.125}Sb, In0.75_{0.75}Ti0.25_{0.25}Sb, and In0.50_{0.50}Ti0.50_{0.50}Sb are presented in Figure 5, Figure 6, and Figure 7. We notice that the majority-spin bands are metallic with respect to the gap located at the Fermi level for the minority-spin channel.

Image not extracted

Figure 5. (Colour online) Spin-polarized band structure obtained with TB-mBJ for In0.875Ti0.125Sb\mathrm{In}_{0.875}\mathrm{Ti}_{0.125}\mathrm{Sb}: (a) majority spin (up) and (b) minority spin (dn). The Fermi level is set to zero (horizontal dotted red line).

Image not extracted

Figure 6. (Colour online) Spin-polarized band structure obtained with TB-mBJ for In0.75Ti0.25Sb\mathrm{In}_{0.75}\mathrm{Ti}_{0.25}\mathrm{Sb}: (a) majority spin (up) and (b) minority spin (dn). The Fermi level is set to zero (horizontal dotted red line).

Image not extracted

Figure 7. (Colour online) Spin-polarized band structure obtained with TB-mBJ for In0.50_{0.50}Ti0.50_{0.50}Sb: (a) majority spin (up) and (b) minority spin (dn). The Fermi level is set to zero (horizontal dotted red line).

Concerning the minority spin, we notice two gaps. The half-metallic ferromagnetic gap GHMFG_{\mathrm{HMF}} and the half-metallic gap (i.e., spin-flip excitation) GHMG_{\mathrm{HM}}. GHMFG_{\mathrm{HMF}} is the energy difference between the valence-band maximum (VBM) and conduction-band minimum (CBM) while GHMG_{\mathrm{HM}} is the smaller energy between the minimum of the conduction band energy compared to the Fermi level and the maximum value of the valence band energy [61]. Figure 8, Figure 9, and Figure 10 shows the spin-polarized band structure of In0.25_{0.25}Ti0.75_{0.75}Sb, In0.125_{0.125}Ti0.875_{0.875}Sb, and TiSb, respectively. It is clear that the structures In1−x_{1-x}Tix_xSb for x=0.75x = 0.75, 0.875, and 1 (TiSb) have a metallic behavior for the two channels (spin up and spin down). The calculated TB-mBJ values of Eg_g, HMF GHMFG_{\mathrm{HMF}}, and HM GHMG_{\mathrm{HM}} gaps of In1−x_{1-x}Tix_xSb for different concentrations are exposed in Table 2 along with other experimental and theoretical data. In order to know the comportment of these alloys around the Fermi level (Fermi energy) EFE_F, we have investigated the total density of states (TDOS) and partial densities of states (PDOS) of the In1−x_{1-x}Tix_xSb material. Such results are illustrated in Figure 11–Figure 17. From these figures, it is found that binary InSb displays a semiconductor alloy, and for In0.875_{0.875}Ti0.125_{0.125}Sb, In0.75_{0.75}Ti0.25_{0.25}Sb, and In0.50_{0.50}Ti0.50_{0.50}Sb systems exhibit a half-metallic ferromagnetic character with spin polarization of 100% by using the following formula given by [62]:

Image not extracted

Figure 8. (Colour online) Spin-polarized band structure obtained with TB-mBJ for In0.25_{0.25}Ti0.75_{0.75}Sb: (a) majority spin (up) and (b) minority spin (dn). The Fermi level is set to zero (horizontal dotted red line).

Image not extracted

Figure 9. (Colour online) Spin-polarized band structure obtained with TB-mBJ for In0.125_{0.125}Ti0.875_{0.875}Sb: (a) majority spin (up) and (b) minority spin (dn). The Fermi level is set to zero (horizontal dotted red line).

Image not extracted

Figure 10. (Colour online) Spin-polarized band structure obtained with TB-mBJ for TiSb: (a) majority spin (up) and (b) minority spin (dn). The Fermi level is set to zero (horizontal dotted red line).

Image not extracted

Figure 11. (Colour online) Spin-polarized total densities of states of InSb. The Fermi level is set to zero (vertical dotted red line).

CompoundGHMFG_{\mathrm{HMF}} (eV)GHMG_{\mathrm{HM}} (eV)EΓ−ΓE^{\Gamma-\Gamma} (eV)MethodBehavior
This workGGA-WC
InSb0.3216
In0.875_{0.875}Ti0.125_{0.125}Sb0.84230.3989HMF
In0.75_{0.75}Ti0.25_{0.25}Sb1.36350.5182HMF
In0.50_{0.50}Ti0.50_{0.50}Sb1.31940.3072HMF
In0.25_{0.25}Ti0.75_{0.75}Sb--Metallic
In0.125_{0.125}Ti0.875_{0.875}Sb--Metallic
TiSb--Metallic
Other calculations
InSb0.24 [29]GGA-WC
0.23, 0.2169, 0.1947, 0.17 [40]Experimental

Table 2. The calculated indirect bandgap for InSb, half-metallic ferromagnetic gap GHMFG_{\mathrm{HMF}} and half-metallic gap GHMG_{\mathrm{HM}} of minority-spin bands for In1−x_{1-x}Tix_xSb at concentrations x=0x = 0, 0.125, 0.25, 0.50, 0.75, 0.875 and 1.

Image not extracted

Figure 17. (Colour online) Spin-polarized (a) total and (b) partial densities of states of TiSb. The Fermi level is set to zero (vertical dotted red line).

P=N↑(EF)−N↓(EF)N↑(EF)+N↓(EF)(5)P = \frac{N \uparrow(E_{\mathrm{F}}) - N \downarrow(E_{\mathrm{F}})}{N \uparrow(E_{\mathrm{F}}) + N \downarrow(E_{\mathrm{F}})} \tag*{(5)}

Here PP is the spin polarization, N↑(EF)N \uparrow(E_{\mathrm{F}}) and N↓(EF)N \downarrow(E_{\mathrm{F}}) are the densities of states of the majority spin and minority spin around the Fermi level, respectively. In accordance with the calculated PP and the total DOS plot and owing to the performance that In0.875_{0.875}Ti0.125_{0.125}Sb, In0.75_{0.75}Ti0.25_{0.25}Sb, and In0.50_{0.50}Ti0.50_{0.50}Sb structures are equal to zero, the spin polarization is 100%, while In0.25_{0.25}Ti0.75_{0.75}Sb, In0.125_{0.125}Ti0.875_{0.875}Sb, and TiSb demonstrates metallic comportment. It evidently appears that the titanium bands are situated at the Fermi level (plot in green). Figure 11 (b), Figure 12 (b), Figure 13 (b), Figure 14 (b), Figure 15 (b), Figure 16 (b), and Figure 17 (b), depict the spin-polarized partial

Image not extracted

Figure 12. (Colour online) Spin-polarized (a) total and (b) partial densities of states of In0.875_{0.875}Ti0.125_{0.125}Sb. The Fermi level is set to zero (vertical dotted red line).

Image not extracted

Figure 13. (Colour online) Spin-polarized (a) total and (b) partial densities of states of In0.75_{0.75}Ti0.25_{0.25}Sb. The Fermi level is set to zero (vertical dotted red line).

Image not extracted

Figure 14. (Colour online) Spin-polarized (a) total and (b) partial densities of states of In0.50_{0.50}Ti0.50_{0.50}Sb. The Fermi level is set to zero (vertical dotted red line).

Image not extracted

Figure 15. (Colour online) Spin-polarized (a) total and (b) partial densities of states of In0.25_{0.25}Ti0.75_{0.75}Sb. The Fermi level is set to zero (vertical dotted red line).

Image not extracted

Figure 16. (Colour online) Spin-polarized (a) total and (b) partial densities of states of In0.125_{0.125}Ti0.875_{0.875}Sb. The Fermi level is set to zero (vertical dotted red line).

electronic density of states for titanium atoms in In1−x_{1-x}Tix_xSb structures. We can observe that the high section of valence bands is formed by the 3d3d (Ti) partially occupied states, and the lowest part of the conduction bands is dominated by the 3d3d (Ti) unoccupied states higher than Fermi level EFE_{\mathrm{F}}.

Magnetic and half-metallicity properties

To explicate the specificity of the effects of the p−dp-d exchange aspect on the magnetic comportment, we calculated the total and local magnetic moments of the Ti, In, and Sb atoms as well as the interstitial sites in the In1−x_{1-x}Tix_xSb structures. Table 3 exposes the total and local magnetic moments of In1−x_{1-x}Tix_xSb for different concentration xx. We can note that the total magnetic moment for each alloy was around 1 μB\mu_{\mathrm{B}}, usually overdue to the local magnetic moment of the Ti atom, and could be mainly attributed to the strong p−dp-d exchange interaction between 3d3d t2gt_{2g} (Ti) and pp (Sb) states. The calculated magnetic moment in interstitial sites in the In1−x_{1-x}Tix_xSb alloys increases with the concentration of Ti. The results also indicate that for In1−x_{1-x}Tix_xSb at all compositions except x=0x=0 (i.e., InSb), the magnetic spins of the atoms between Ti and Sb and between Sb and In have opposite signs, signifying the antiparallel induced ferromagnetic interaction between Ti and Sb and between Sb and In.

CompoundTotal (μB\mu_{\mathrm{B}})Ti (μB\mu_{\mathrm{B}})In (μB\mu_{\mathrm{B}})Sb (μB\mu_{\mathrm{B}})Interstitial (μB\mu_{\mathrm{B}})
InSb0-000
In0.875_{0.875}Ti0.125_{0.125}Sb10.85840.0023−0.0164-0.01640.1925
In0.75_{0.75}Ti0.25_{0.25}Sb10.84620.0046−0.0266-0.02660.3864
In0.50_{0.50}Ti0.50_{0.50}Sb10.86410.0151−0.1164-0.11640.8054
In0.25_{0.25}Ti0.75_{0.75}Sb10.80630.0343−0.0635-0.06351.4459
In0.125_{0.125}Ti0.875_{0.875}Sb10.84770.0416−0.1295-0.12951.6442
TiSb10.70123-−0.04942-0.049420.1800

Table 3. Calculated total and local magnetic moments per Ti atom of the relevant Ti, In, and Sb atoms and in the interstitial sites (in Bohr magneton BB) for In1−x_{1-x}Tix_xSb at concentrations x=0x = 0, 0.125, 0.25, 0.50, 0.75, 0.875 and 1.

Conclusion

In this paper, we used the Full-Potential Linearized Augmented Plane Wave (FP-LAPW+lo) method to predict the structural, electronic, and magnetic properties of the substitutional doping of Titanium on the binary InSb alloy. In0.875_{0.875}Ti0.125_{0.125}Sb, In0.75_{0.75}Ti0.25_{0.25}Sb, In0.50_{0.50}Ti0.50_{0.50}Sb, In0.25_{0.25}Ti0.75_{0.75}Sb, and In0.125_{0.125}Ti0.875_{0.875}Sb structures were evaluated. The calculated formation and cohesive energy demonstrates that In0.875_{0.875}Ti0.125_{0.125}Sb, In0.75_{0.75}Ti0.25_{0.25}Sb, In0.50_{0.50}Ti0.50_{0.50}Sb, In0.25_{0.25}Ti0.75_{0.75}Sb, and In0.125_{0.125}Ti0.875_{0.875}Sb alloys are stable and can be synthesized. We used GGA-PBEsol approximation to predict the ground-state properties. The calculated structural parameters of InSb are in good agreement with the available theoretical and experimental data. GGA-PBEsol coupled with (TB-mBJ) of Tran-Blaha modified Becke-Johnson approximation was used to estimate electronic and magnetic properties. We demonstrated that In0.875_{0.875}Ti0.125_{0.125}Sb, In0.75_{0.75}Ti0.25_{0.25}Sb, and In0.50_{0.50}Ti0.50_{0.50}Sb are half-metallic ferromagnetic structures with a spin polarization of 100% at the Fermi level, while In0.25_{0.25}Ti0.75_{0.75}Sb, and In0.125_{0.125}Ti0.875_{0.875}Sb present a metallic comportment. The total magnetic moments are 1 μB\mu_{\mathrm{B}} for all compounds. The investigation of magnetic properties demonstrates that the p−dp-d exchange systems operate in stabilizing ferromagnetic state configuration, and are the origin of a low magnetic moment in the investigated alloys. According to our bibliographic research, there are no earlier theoretical or experimental studies on the In1−x_{1-x}Tix_xSb materials. Thus, we hope that our results serve as a reference for future theoretical and experimental research.

Дослідження структурних, магнітних і електронних властивостей та напівметалічності твердих розчинів In1−xTixSb\mathrm{In}_{1-x}\mathrm{Ti}_{x}\mathrm{Sb} на основі методу функціоналу густини

С. Амрані; М. Бербер; М. Мебрек

З метою з’ясування впливу заміщення в легованому атомами Ti сплаві InSb проведено першопринципні розрахунки в рамках методу лінеаризованих розширених плоских хвиль з повним потенціалом (ЛРПХзПП). З використанням узагальненого градієнтного наближення Пердью-Бурке-Ернцергофа для твердих тіл (УГН-ПБЕтт) в покращеному підході Тран-Блаха з модифікацією Бека-Джонсона (ТБ-мБД) передбачено структурні, електронні і магнітні властивості сполук In1−xTixSb\mathrm{In}_{1-x}\mathrm{Ti}_{x}\mathrm{Sb} з концентраціями x=0x = 0, 0.125, 0.25, 0.50, 0.75, 0.875$ та 1. Розраховані значення сталих ґратки добре узгоджуються з наявними теоретичними та експериментальними даними. Як показують розрахунки, усі структури є енергетично стійкими. Легування заміщення перетворює іонний характер вихідної сполуки InSb на напівметалічну феромагнітну поведінку для концентрацій x=0x = 0, 0.125, 0.25 і 0.50, зі 100% спіновою поляризацією на рівні Фермі та на металічну для In0.25Ti0.75Sb\mathrm{In}_{0.25}\mathrm{Ti}_{0.75}\mathrm{Sb} і In0.125Ti0.875Sb\mathrm{In}_{0.125}\mathrm{Ti}_{0.875}\mathrm{Sb}. Оціночні значення повних магнітних моментів становлять приблизно 1 μB\mu_\mathrm{B}. In0.875Ti0.125Sb\mathrm{In}_{0.875}\mathrm{Ti}_{0.125}\mathrm{Sb}, In0.75Ti0.25Sb\mathrm{In}_{0.75}\mathrm{Ti}_{0.25}\mathrm{Sb}, та In0.50Ti0.50Sb\mathrm{In}_{0.50}\mathrm{Ti}_{0.50}\mathrm{Sb} демонструють напівметалічну феромагнітну поведінку та потенційно можуть використовуватися в спінтроніці.

References

  1. [1]Volkov B. A., Mnatsakanov T. T., Zh. Eksp. Teor. Fiz., 1978, 75, 563.
  2. [2]Yakovlev D. R., Ossau W., Introduction to the Physics of Diluted Magnetic Semiconductors, Springer, Berlin, 2010.
  3. [3]Laroussi A., Berber M., Mokaddem A., Doumi B., Abid H., Boudali A., Acta Phys. Pol. A, 2019, 135, 451, doi:10.12693/APHYSPOLA.135.451.DOI
  4. [4]Laroussi A., Berber M., Doumi B., Mokaddem A., Abid H., Boudali A., Bahloul H., Mоуjri H., Appl. Phys. A, 2019, 125, No. 10, 1–13, doi:10.1007/s00339-019-2973-2.DOI
  5. [5]Berber M., Doumi B., Mokaddem A., Mogulkoc Y., Sayede A., Tadjer A., J. Comput. Electron., 2017, 16, No. 3, 542–547, doi:10.1007/s10825-017-1038-z.DOI
  6. [6]Berber M., Doumi B., Mokaddem A., Mogulkoc Y., Sayede A., Tadjer A., J. Electron. Mater., 2018, 47, No. 1, 449–456, doi:10.1007/s11664-017-5793-1.DOI
  7. [7]Bahloul H., Mokaddem A., Doumi B., Berber M., Boudali A., J. Supercond. Novel Magn., 2019, 32, No. 7, 2185–2192, doi:10.1007/s10948-018-4948-5.DOI
  8. [8]Boutaleb M., Hsini M., Zemouli M., Berber M., Tadjer A., Int. J. Comput. Mater. Sci. Eng., 2021, 10, No. 1, 2150006, doi:10.1142/S2047684121500068.DOI
  9. [9]Bouziani I., Benhouria Y., Essaoudi I., Ainane A., Ahuja R., Mater. Sci. Eng., B, 2020, 253, 114484, doi:10.1016/j.mseb.2019.114484.DOI
  10. [10]Khan M. S., Shi L., Zou B., Ali S., Comput. Mater. Sci., 2020, 174, 109491, doi:10.1016/j.commatsci.2019.109491.DOI
  11. [11]Marquina J., Quintero E., Ruette F., Bentancurt Y., Chin. J. Phys., 2020, 63, 63–69, doi:10.1016/j.cjph.2019.09.037.DOI
  12. [12]Moniri M. E. A., Bahnes A., Boukourt A., Requig A. B., Mouchaal Y., J. Magn. Magn. Mater., 2020, 497, 166067, doi:10.1016/j.jmmm.2019.166067.
  13. [13]Korichi K., Doumi B., Mokaddem A., Sayede A., Tadjer A., Philos. Mag., 2020, 100, No. 9, 1172–1190, doi:10.1080/14786435.2020.1723812.DOI
  14. [14]Hamidane N., Baaziz H., Ocak H. Y., Baddari K., Uğur Ş., Uğur G., Charifi Z., J. Supercond. Novel Magn., 2020, 33, No. 10, 3263–3272, doi:10.1007/s10948-020-05527-w.DOI
  15. [15]Maftouh A., Rami R., Drissi L. B., El Fatni O., Ahl Laamara R., Solid State Commun., 2021, 339, 114482, doi:10.1016/j.ssc.2021.114482.DOI
  16. [16]Kumar A., Karr M., Sati P. C., Srivastava M. K., Ghosh S., Kumar S., Curr. Appl Phys., 2021, 32, 24–35, doi:10.1016/j.cap.2021.09.002.DOI
  17. [17]Abo-Naf S. M., Ibrahim S., Marzouk M. A., Appl. Phys. A, 2021, 127, No. 6, 1–11, doi:10.1007/s00339-021-04583-w.
  18. [18]Yehia M., Labib Sh., Ismail S. M., J. Inorg. Organomet. Polym. Mater., 2021, 31, 4491–4503, doi:10.1007/s10904-021-02051-9.DOI
  19. [19]Zhao X., Liang H., Chen Y., Chen X., Zhang W., Wang J., Zhang G., Belotelov V. I., Song Y., J. Mater. Chem. C, 2021, 9, No. 13, 4619–4627, doi:10.1039/D0TC06026G.DOI
  20. [20]Cho A. Y., Arthur J. R., Prog. Solid. State Ch., 1975, 10, 157–191, doi:10.1016/0079-6786(75)90005-9.DOI
  21. [21]Sandhu A., Sanbonsugi H., Shibasaki I., Abe M., Handa H., Jpn. J. Appl. Phys., 2004, 43, No. 7A, L868, doi:10.1143/JJAP.43.L868.DOI
  22. [22]Nilsson H. A., Caroff P., Thelander C., Larsson M., Wagner J. B., Wernersson L. E., Samuelson L., Xu H. Q., Nano Lett., 2009, 9, No. 9, 3151–3156, doi:10.1021/nl901333a.DOI
  23. [23]Kuo C. H., Wu J. M., Lin S. J., Chang W. C., Nanoscale Res. Lett., 2013, 8, No. 1, 327, doi:10.1186/1556-276X-8-327.DOI
  24. [24]Minamoto M. T., Allen C. M., Solid-State Electron., 1962, 5, No. 4, 263–266, doi:10.1016/0038-1101(62)90107-7.DOI
  25. [25]Maffitt K. N., Mueller R. K., J. Appl. Phys., 1964, 35, No. 5, 1563–1564, doi:10.1063/1.1713667.DOI
  26. [26]Hattori K., Yuito M., Amakusa T., Phys. Status Solidi A, 1982, 73, No. 1, 157–164, doi:10.1002/pssa.2210730120.DOI
  27. [27]Kimukin I., Biyikli N., Ozbay E., J. Appl. Phys., 2003, 94, No. 8, 5414–5416, doi:10.1063/1.1611286.DOI
  28. [28]Ashley T., Buckle L., Datta S., Emeny M. T., Hayes D. G., Hilton K. P., Jefferies R., Martin T., Phillips T. J., Wallis D. J., Wilding P. J., Chau R., Electron. Lett., 2007, 43, No. 14, doi:10.1049/el:20071335.DOI
  29. [29]Singh J., Poolla R., J. Mater. Sci.: Mater. Electron., 2017, 28, No. 18, 13716–13726, doi:10.1007/s10854-017-7216-8.DOI
  30. [30]Fawcett W., Ruch J. G., Appl. Phys. Lett., 1969, 15, No. 11, 368–370, doi:10.1063/1.1652863.DOI
  31. [31]Ashley T., Dean A. B., Elliott C. T., Pryce G. J., Johnson A. D., Willis H., Appl. Phys. Lett., 1995, 66, No. 4, 481–483, doi:10.1063/1.114063.DOI
  32. [32]Raj ska D., Brzózka A., Marciszko-Wiąckowska M., Marzec M. M., Chlebda D., Hnida-Gut K. E., Sulka G. D., Appl. Surf. Sci., 2021, 537, 147715, doi:10.1016/j.apsusc.2020.147715.
  33. [33]Yamaguchi S., Matsumoto T., Yamazaki J., Kaiwa N., Yamamoto A., Appl. Phys. Lett., 2005, 87, No. 20, 201902, doi:10.1063/1.2130390.DOI
  34. [34]Okamoto A., Shibasaki I., J. Cryst. Growth, 2003, 251, No. 1–4, 560–564, doi:10.1016/s0022-0248(02)02448-x.DOI
  35. [35]Kochura A., Marenkin S., Novodvorsky O., Mikhalevsky V., Davidov A., Shakhov M., Lahderanta E., Zakhvalinskii V., Kuzmenko A., EPJ Web of Conferences, 2018, 185, 06003, doi:10.1051/epjconf/201818506003.DOI
  36. [36]You J. Y., Gu B., Maekawa S., Su G., Phys. Rev. B, 2020, 102, No. 9, 094432, doi:10.1103/PhysRevB.102.094432.DOI
  37. [37]Mir S. A., Gupta D. C., J. Magn. Magn. Mater., 2020, 493, 165722, doi:10.1016/j.jmmm.2019.165722.DOI
  38. [38]Berber M., Bouzouira N. E., Abid H., Boudali A., Moujri H., Rev. Mex. de Fis., 66, No. 5, 604–609, doi:10.31349/RevMexFis.66.604.
  39. [39]Pappert K., Schmidt M. J., Hümpfner S., Rüster C., Schott G. M., Brunner K., Gould C., Schmidt G., Molen kamp L. W., Phys. Rev. Lett., 2006, 97, No. 18, 186402, doi:10.1103/PhysRevLett.97.186402.DOI
  40. [40]Onho H., Shen A., Matsukura F., Oiwa A., Endo A., Katsumoto S., Iye Y., Appl. Phys. Lett., 1996, 69, No. 3, 363–365, doi:10.1063/1.118061.
  41. [41]Sato K., Katayama-Yoshida H., Jpn. J. Appl. Phys., 2000, 39, No. 6B, L555, doi:10.1143/JJAP.39.L555.DOI
  42. [42]Ruderman M. A., Kittel C., Phys. Rev., 1954, 96, No. 1, 99, doi:10.1103/PhysRev.96.99.DOI
  43. [43]Yosida K., Phys. Rev., 1957, 106, No. 5, 893, doi:10.1103/PhysRev.106.893.DOI
  44. [44]Wong K. M., Alay-e-Abbas S. M., Shaukat A., Fang Y., Lei Y., J. Appl. Phys., 2013, 113, No. 1, 014304, doi:10.1063/1.4772647.DOI
  45. [45]Khalil B., Naji S., Labrim H., Bhihi M., El Hachimi A. G., Lakhal M., Belhaj A., Benyoussef A., El Kenz A., J. Supercond. Novel Magn., 2014, 27, No. 1, 203–208, doi:10.1007/s10948-013-2241-1.
  46. [46]Berri S., Kouriche A., Maouche D., Zerarga F., Attallah M., Mater. Sci. Semicond. Process., 2015, 38, 101–106, doi:10.1016/j.mssp.2015.04.016.DOI
  47. [47]Sjöstedt E., Nordström L., Singh D. J., Solid State Commun., 2000, 114, No. 1, 15–20, doi:10.1016/S0038-1098(99)00577-3.DOI
  48. [48]Blaha P., Schwarz K., Madsen G. K. H., Kvasnicka D., Luitz J., Laskowski R., Tran F., Marks L. D., WIEN2k: An Augmented Plane Wave Plus Local Orbitals Program for Calculating Crystal Properties, Vienna University of Technology, Austria, 2018.
  49. [49]Perdew J. P., Burke K., Ernzerhof M., Phys. Rev. Lett., 1996, 77, No. 18, 3865, doi:10.1103/PhysRevLett.77.3865.DOI
  50. [50]Koller D., Tran F., Blaha P., Phys. Rev. B, 2011, 83, No. 19, 195134, doi:10.1103/PhysRevB.83.195134.DOI
  51. [51]Koller D., Tran F., Blaha P., Phys. Rev. B, 2012, 85, No. 15, 155109, doi:10.1103/PhysRevB.85.155109.DOI
  52. [52]Tran F., Blaha P., Phys. Rev. Lett., 2009, 102, No. 22, 226401, doi:10.1103/PhysRevLett.102.226401.DOI
  53. [53]Vegard L., J. Phys., 1921, 5, No. 5, 393–395.
  54. [54]Breivik M., Nilsen T. A., Finland B. O., J. Cryst. Growth, 2013, 381, 165–168, doi:10.1016/j.jcrysgro.2013.06.034.DOI
  55. [55]Adachi S., In: Optical Constants of Crystalline and Amorphous Semiconductors, Springer, Boston, MA, 1999, 268–278, doi:10.1007/978-1-4615-5247-5_27.
  56. [56]Liu T. S., Peretti E. A., JOM, 1951, 3, No. 9, 791–791, doi:10.1007/BF03397373.DOI
  57. [57]Orton J. W., Semiconductors and the Information Revolution: Magic Crystals That Made IT Happen, Academic Press, 2009.
  58. [58]Birch F., Phys. Rev., 1947, 71, No. 11, 809, doi:10.1103/PhysRev.71.809.DOI
  59. [59]Reunchan P., Umezawa N., Ouyang S., Ye J., Phys. Chem. Chem. Phys., 2012, 14, No. 6, 1876–1880, doi:10.1039/C2CP23348G.DOI
  60. [60]Liu Y., Zhou W., Wu P., J. Appl. Phys., 2017, 121, No. 7, 075102, doi:10.1063/1.4976812.DOI
  61. [61]Gao G. Y., Yao K. L., Şaşıoğlu E., Sandratskii L. M., Liu Z. L., Jiang J. L., Phys. Rev. B, 2007, 75, No. 17, 174442, doi:10.1103/PhysRevB.75.174442.DOI
  62. [62]Bai J., Raulot J. M., Zhang Y., Esling C., Zhao X., Zuo L., Appl. Phys. Lett., 2011, 98, No. 16, 164103, doi:10.1063/1.3582239.DOI

Paper details

vlnc:W_z8vz59nm
Version
v1 · latest
Published
Fresh — added to the Hub within the last 30 days
Added
License
CC BY 4.0
Usage

views · 0

downloads · 0

A view counts once per browser per day, a download each time the PDF is requested.

  • Physics and Astronomy

Not recorded for this paper

View statement
Looking for related papers…
Contents