Local structural distortions drive magnetic molecular field in compositionally complex spinel oxide

Abstract

Understanding how local distortions determine the functional properties of high entropy materials, containing five or more elements at a crystallographic site, is an open challenge. We address this for a compositionally complex spinel oxide (Mn0.2_{0.2}Co0.2_{0.2}Ni0.2_{0.2}Cu0.2_{0.2}Zn0.2_{0.2})Cr2_2O4_4 (A5A^5Cr2_2O4_4). By comparatively examining extended X-ray absorption fine structure on A5A^5Cr2_2O4_4 and its parent counterparts AACr2_2O4_4 along with density functional theory calculations for multiple configurations, we find that the element-specific distortions go beyond the first neighbor. Specifically, the strong Jahn-Teller distortion present in CuCr2_2O4_4 is found to be completely suppressed in A5A^5Cr2_2O4_4. Instead, there is a broad distribution of Cu-O and Cu-Cr bond distances while other AA-O distances acquire certain specific values. This study demonstrates the additional flexibility of a cationic sublattice in maintaining a uniform long-range structure, in contrast to previous reports showing only the accommodative anionic sublattice. Remarkably, despite the presence of multiple magnetic ions and variable bond lengths, the mean field magnetic interactions of A5A^5Cr2_2O4_4 exhibit a striking resemblance to those of NiCr2_2O4_4. This compelling observation originates from the comparability of bond lengths around Cr in both materials. Our study paves the way for a deeper understanding of the impact of local structural distortions in compositionally complex quantum materials, enabling the targeted design with tailored properties.

The periodic arrangement of atoms/ions/molecules within crystalline materials is the backbone of their diverse electronic, magnetic, and topological properties. Conventionally, crystalline materials are synthesized based on the principle of enthalpy minimization. However, in recent years, there has been a surge of interest in high-entropy materials that break this paradigm, where high configurational entropy drives structure formation [1, 2, 3, 4, 5, 6, 7]. Originally introduced for multicomponent alloys [8, 9], this concept was extended to oxide ceramics in 2015 by demonstrating the stabilization of Mg0.2Co0.2Ni0.2Cu0.2Zn0.2O\mathrm{Mg}_{0.2}\mathrm{Co}_{0.2}\mathrm{Ni}_{0.2}\mathrm{Cu}_{0.2}\mathrm{Zn}_{0.2}\mathrm{O} in a rock-salt structure [10]. Since then, high entropy oxides (HEOs) have been synthesized with a variety of structures, such as fluorites (AO2−δ\mathrm{AO}_{2-\delta}) [11], perovskites (ABO3\mathrm{ABO}_{3}) [12, 13, 14, 15], spinels (AB2O4\mathrm{AB}_{2}\mathrm{O}_{4}) [16, 17, 18], and pyrochlores (A2B2O7\mathrm{A}_{2}\mathrm{B}_{2}\mathrm{O}_{7}) [19, 20, 21], where at least one of the crystallographic sites is occupied by five or more elements in equal or nearly equal atomic fractions. Despite not all being entropy-stabilized [5], these compositionally complex oxides (CCOs) exhibit interesting properties beyond their single element counterparts and hold potential for applications such as energy storage, catalysis, and microwave absorption, etc. [22, 23, 24, 25, 26, 27, 28].

Local lattice distortions [Figure 1(a),(Figure 1b)] in high entropy alloys (HEAs), a critical factor influencing their mechanical and physical properties, remain an open issue [29]. The presence of multiple sublattices adds further challenges in comprehending the interplay among disorder, distortions, and electronic/magnetic properties in CCO [30]. In conventional oxides with low disorder, distortions around individual cations are generally related to their ionic radii, coordination numbers, and oxidation states, which control electron hopping and magnetic exchange interaction strength. The local distortions around each cation within the disordered sublattice of CCO are expected to be highly variable and likely to deviate significantly from the average long-range structure probed by the diffraction technique. It is also necessary to determine the extent of this local distortion variation across neighboring elements and how it affects the material’s properties. To address these issues, we employ the extended X-ray absorption fine structure (EXAFS) technique, in conjunction with density functional theory (DFT) calculations. EXAFS is an element-specific method used to study the local chemical distribution (length scale up to ∼5-6 A˚\sim5\text{-}6\,\mathrm{\AA}) around particular atoms [31, 32, 33]. EXAFS spectra are specifically sensitive to the coordination number, bond distances, and atomic species surrounding the absorber, providing a relatively simple way to understand the local structural distortion. Interestingly, EXAFS studies have shown that the variation in cation-specific bond lengths is confined only to the first coordination shell in the case of rock-salt HEOs [34, 35]. This work rigorously investigates the crucial influence of local structural distortions on the magnetic behavior of a spinel oxide within a compositionally complex setting.

Long-range structural characterization showing BCC lattice structures, compositionally complex spinel structure, Rietveld-refined XRD data, lattice parameters, and Raman spectra

Figure 1. Long-range structural characterization. Schematic to show (a) body centered cubic (BCC) lattice structure of a pure metal, and (b) a distorted BCC structure for a high entropy alloy with five five different elements present in near equal fraction. c Schematic of A5Cr2O4A^{5}\mathrm{Cr}_{2}\mathrm{O}_{4} with cubic spinel structure having Cr at the octahedral site and AA (= Mn, Co, Ni, Cu and Zn) at the tetrahedral site. d Rietveld refined XRD data for CuCr2O4\mathrm{CuCr}_{2}\mathrm{O}_{4} and ZnCr2O4\mathrm{ZnCr}_{2}\mathrm{O}_{4} along with A5Cr2O4A^{5}\mathrm{Cr}_{2}\mathrm{O}_{4}. e The lattice parameters for the parent compounds and A5Cr2O4A^{5}\mathrm{Cr}_{2}\mathrm{O}_{4} as obtained from the Rietveld analysis. The parameter aa in the tetragonal phases of NiCr2O4\mathrm{NiCr}_{2}\mathrm{O}_{4} and CuCr2O4\mathrm{CuCr}_{2}\mathrm{O}_{4} have been multiplied by 2\sqrt{2} for ease of comparison. f Raman spectra of A5Cr2O4A^{5}\mathrm{Cr}_{2}\mathrm{O}_{4} has been compared with cubic ZnCr2O4\mathrm{ZnCr}_{2}\mathrm{O}_{4} and tetragonal CuCr2O4\mathrm{CuCr}_{2}\mathrm{O}_{4}. The allowed Raman modes for cubic and tetrogonal spinels are A1g+Eg+3F2gA_{1g}+E_{g}+3F_{2g}, and 2A1g+B1g+3B2g+4Eg2A_{1g}+B_{1g}+3B_{2g}+4E_{g}, respectively [36, 37]. In our experiments, we found 4 modes for cubic and 8 modes for tetragonal compounds.

The normal AB2O4AB_{2}\mathrm{O}_{4} spinel consists of a diamond lattice formed by the tetrahedrally coordinated AA site and a pyrochlore lattice formed by the octahedrally coordinated BB site [Fig. 1(c)]. The spinel family has been extensively studied for over a century due to the observation of various phenomena, such as magnetic ordering, frustrated magnetism, orbital ordering, charge ordering, metal-insulator transitions, etc [38]. This study centers on the ACr2O4\mathrm{A}\mathrm{Cr}_{2}\mathrm{O}_{4} family, a group of normal spinel compounds that display diverse low-temperature magnetic behaviors. Interestingly, their Curie-Weiss temperatures (θCW\theta_{\mathrm{CW}}), ranging from -400 K to 200 K, directly correlate with the Cr-Cr separation [39]. In this work, we have synthesized (Mn0.2Co0.2Ni0.2Cu0.2Zn0.2)Cr2O4(\mathrm{Mn}_{0.2}\mathrm{Co}_{0.2}\mathrm{Ni}_{0.2}\mathrm{Cu}_{0.2}\mathrm{Zn}_{0.2})\mathrm{Cr}_{2}\mathrm{O}_{4} (hereafter referred to as A5Cr2O4\mathrm{A}^{5}\mathrm{Cr}_{2}\mathrm{O}_{4}). The individual members MnCr2O4\mathrm{MnCr}_{2}\mathrm{O}_{4} and CoCr2O4\mathrm{CoCr}_{2}\mathrm{O}_{4} are cubic and become ferrimagnetic at TcT_{\mathrm{c}} values of 41 K and 93 K, respectively [40, 41, 42, 43]. Additionally, they exhibit multiferroic behavior below 18 K and 27 K [40, 41, 42, 43]. Due to the Jahn-Teller activity of the Ni2+\mathrm{Ni}^{2+} and Cu2+\mathrm{Cu}^{2+} ions, NiCr2O4\mathrm{NiCr}_{2}\mathrm{O}_{4} and CuCr2O4\mathrm{CuCr}_{2}\mathrm{O}_{4} undergo cubic to tetragonal transitions below 310 K and 853 K, respectively. They transform into an orthorhombic phase at 65 K and 125 K, respectively, accompanied by a ferrimagnetic transition [44]. On the other hand, ZnCr2O4\mathrm{ZnCr}_{2}\mathrm{O}_{4} is cubic at room temperature and exhibits an antiferromagnetic ordering transition below 12 K [45].

In the present work, we probe the modification of the local structure of A5Cr2O4\mathrm{A}^{5}\mathrm{Cr}_{2}\mathrm{O}_{4} compared to that of its five undoped counterparts (ACr2O4\mathrm{ACr}_{2}\mathrm{O}_{4}, A=Mn,Co,Ni,Cu,ZnA = \mathrm{Mn}, \mathrm{Co}, \mathrm{Ni}, \mathrm{Cu}, \mathrm{Zn}) at room temperature. X-ray diffraction (XRD), Raman spectroscopy, and X-ray absorption spectroscopy (XAS) of the transition metal L3,2L_{3,2} edges confirmed the desired normal spinel structure of A5Cr2O4\mathrm{A}^{5}\mathrm{Cr}_{2}\mathrm{O}_{4} with cubic symmetry. Our comprehensive EXAFS measurements and DFT based calculations revealed the element-specific local structural distortions in A5Cr2O4\mathrm{A}^{5}\mathrm{Cr}_{2}\mathrm{O}_{4} persist beyond the first neighbor. Interestingly, the Jahn-Teller distortions typically observed in the CuCr2O4\mathrm{CuCr}_{2}\mathrm{O}_{4} are absent in A5Cr2O4\mathrm{A}^{5}\mathrm{Cr}_{2}\mathrm{O}_{4}. Rather, CuO4\mathrm{CuO}_{4} units are highly flexible to accommodate local distortions while maintaining a uniform long-range cubic structure. We further show that the near-identical Cr-O and Cr-Cr bond lengths in A5Cr2O4\mathrm{A}^{5}\mathrm{Cr}_{2}\mathrm{O}_{4} and NiCr2O4\mathrm{NiCr}_{2}\mathrm{O}_{4} are responsible for their similar θCW\theta_{\mathrm{CW}}.

Results

Synthesis and global structural symmetry: The synthesis of polycrystalline samples of five parent compounds ACr2O4\mathrm{ACr}_{2}\mathrm{O}_{4} (A=Mn,Co,Ni,CuA = \mathrm{Mn}, \mathrm{Co}, \mathrm{Ni}, \mathrm{Cu} and Zn\mathrm{Zn}) and A5Cr2O4\mathrm{A}^{5}\mathrm{Cr}_{2}\mathrm{O}_{4} was carried out using a conventional solid-state synthesis route (details are provided in the Methods section). The powder X-ray diffraction (XRD) pattern of A5Cr2O4\mathrm{A}^{5}\mathrm{Cr}_{2}\mathrm{O}_{4} at room temperature is compared with that of two parent members, tetragonal CuCr2O4\mathrm{CuCr}_{2}\mathrm{O}_{4} and cubic ZnCr2O4\mathrm{ZnCr}_{2}\mathrm{O}_{4}, in Figure 1(d). Similar to ZnCr2O4\mathrm{ZnCr}_{2}\mathrm{O}_{4}, the diffraction pattern of A5Cr2O4\mathrm{A}^{5}\mathrm{Cr}_{2}\mathrm{O}_{4} can be indexed and refined with a normal spinel structure with cubic symmetry having a space group of Fd3ˉmFd\bar{3}m (space group number: 227). The diffraction patterns and structural information obtained from the refinement of all six compounds are shown in the Supplementary (Table S1 and Fig. S1). The lattice constants and lattice volumes of five parent

members and A5Cr2O4A^{5}\mathrm{Cr}_{2}\mathrm{O}_{4} at room temperature are shown in Figure 1(e). For comparison, the lattice constant aa of the tetragonal members NiCr2O4\mathrm{NiCr}_{2}\mathrm{O}_{4} and CuCr2O4\mathrm{CuCr}_{2}\mathrm{O}_{4} is multiplied by 2\sqrt{2} (see Supplementary Fig. S2). The trend in lattice parameters and volume can be understood by considering the ionic radii of A2+A^{2+} ions. The average ionic radii (0.592 Å) of the AA-site for A5Cr2O4A^{5}\mathrm{Cr}_{2}\mathrm{O}_{4} are closer to those of Zn2+\mathrm{Zn}^{2+} (0.60 Å) and Co2+\mathrm{Co}^{2+} (0.58 Å) [ionic radii of Mn2+\mathrm{Mn}^{2+}: 0.66 Å, Ni2+\mathrm{Ni}^{2+}: 0.55 Å, and Cu2+\mathrm{Cu}^{2+}: 0.57 Å] [48], leading to similar unit cell volumes of A5Cr2O4A^{5}\mathrm{Cr}_{2}\mathrm{O}_{4} and ACr2O4A\mathrm{Cr}_{2}\mathrm{O}_{4} (A=A= Co and Zn). Although NiCr2O4\mathrm{NiCr}_{2}\mathrm{O}_{4} is tetragonal, the Jahn-Teller distortion is very small at 300 K, and the unit cell volume is very similar to A5Cr2O4A^{5}\mathrm{Cr}_{2}\mathrm{O}_{4}. It can also be inferred from Figure 1(e) that the Mn and Cu ions are likely to experience internal stress (compressive for Mn and tensile for Cu) when introduced into A5Cr2O4A^{5}\mathrm{Cr}_{2}\mathrm{O}_{4}, leading to local structural distortions.

The Raman spectrum of A5Cr2O4A^{5}\mathrm{Cr}_{2}\mathrm{O}_{4} has been further compared with cubic ZnCr2O4\mathrm{ZnCr}_{2}\mathrm{O}_{4} and tetragonal CuCr2O4\mathrm{CuCr}_{2}\mathrm{O}_{4} at Figure 1(f). ZnCr2O4\mathrm{ZnCr}_{2}\mathrm{O}_{4} shows F2g(1)F_{2g}(1), F2g(2)F_{2g}(2), F2g(3)F_{2g}(3) and A1gA_{1g} modes at 185 cm−1^{-1}, 511 cm−1^{-1}, 604 cm−1^{-1}, 684 cm−1^{-1}, respectively, similar to earlier report [36]. Due to the lower symmetry, CuCr2O4\mathrm{CuCr}_{2}\mathrm{O}_{4} exhibits additional Raman modes [37]. The similarity between the Raman spectra of A5Cr2O4A^{5}\mathrm{Cr}_{2}\mathrm{O}_{4} and ZnCr2O4\mathrm{ZnCr}_{2}\mathrm{O}_{4} further establishes its cubic symmetry. More significantly, we observe shifts and broadening of Raman modes, providing direct evidence of substantial lattice distortions within the compositionally complex A5Cr2O4A^{5}\mathrm{Cr}_{2}\mathrm{O}_{4} [49], which we probe further in detail using element-sensitive EXAFS technique.

Transition metal valency and crystal field environment: Prior to investigating local distortions, we determine the location of cations within octahedral and tetrahedral sites. For this, we carried out element-specific XAS experiments on the L3,2L_{3,2} edges of transition metal ions because the XAS spectral line shape for the 2p63dn→2p53dn+12p^{6}3d^{n}\rightarrow2p^{5}3d^{n+1} transition is strongly dependent on the valency, spin character of the initial state and crystal field environment of the system [50]. The XAS spectra for the L3,2L_{3,2} edges of Cr, Mn, Co, Ni, and Cu in A5Cr2O4A^{5}\mathrm{Cr}_{2}\mathrm{O}_{4}, recorded in total electron yield mode, were compared with those of the corresponding parent compounds, as shown in Figure 2 (a)-(Figure 2e). In all parent ACr2O4A\mathrm{Cr}_{2}\mathrm{O}_{4} compounds, the cations A2+A^{2+} occupy the tetrahedral site, while Cr3+\mathrm{Cr}^{3+} occupies the octahedral site [38]. It is evident from Figure 2 (a)-(Figure 2e) that the spectra of Cr, Mn, Co, and Ni for A5Cr2O4A^{5}\mathrm{Cr}_{2}\mathrm{O}_{4} look exactly similar to the corresponding edges of the parent compounds [46, 47, 51]. Although the main features of Cu L3,2L_{3,2} XAS for A5Cr2O4A^{5}\mathrm{Cr}_{2}\mathrm{O}_{4} are quite similar to those of the parent CuCr2O4\mathrm{CuCr}_{2}\mathrm{O}_{4}, the features at approximately 933.9 eV and 953.7 eV are more intense. This slight difference may be attributed to the differences in crystal field parameters due to the variation in local structures around Cu (demonstrated in the latter part of the manuscript).

Figure 2. Determination of oxidation state using X-ray absorption spectroscopy. a Cr L3,2L_{3,2} edge in MnCr2_2O4_4 and A5^{5}Cr2_2O4_4. b Mn L3,2L_{3,2} edge in MnCr2_2O4_4 and A5^{5}Cr2_2O4_4. c Co L3,2L_{3,2} edge in CoCr2_2O4_4 and A5^{5}Cr2_2O4_4. d Ni L3,2L_{3,2} edge in NiCr2_2O4_4 and A5^{5}Cr2_2O4_4. e Cu L3,2L_{3,2} edge in CuCr2_2O4_4 and A5^{5}Cr2_2O4_4. The spectra of Cr and Mn for MnCr2_2O4_4 is taken from Ref. 46. The spectra of Co for CoCr2_2O4_4 is adapted from Ref. 47. f Spin configurations of Cr, Mn, Co, Ni, Cu, and Zn cations in A5^{5}Cr2_2O4_4. The energy gap between t2gt_{2g} (t2t_2) and ege_g (ee) is not according to the scale.

Overall, our XAS measurements confirmed that the compound has a normal spinel structure, similar to that of its parent counterparts. Figure 2(f) shows the expected spin configurations for each of the cations of A5Cr2O4\mathrm{A}^{5}\mathrm{Cr}_{2}\mathrm{O}_{4}, according to the oxidation state found by XAS. This is further corroborated by the Curie–Weiss analysis of magnetic susceptibility, which is discussed in the later section of the manuscript.

Investigation of local distortions: To investigate the local structural distortions around each cation in A5Cr2O4\mathrm{A}^{5}\mathrm{Cr}_{2}\mathrm{O}_{4}, we analyzed EXAFS data for each of the metal KK-edge in A5Cr2O4\mathrm{A}^{5}\mathrm{Cr}_{2}\mathrm{O}_{4} as well as all the parent compounds (the details of experiment and data analysis have been provided in Method section). Supplementary Fig. S3 displays XANES (X-ray absorption near edge structure) region of the KK-edge XAS spectra, confirming octahedral coordination of Cr and tetrahedral coordination of AA elements. The KK edge EXAFS spectra are shown in Figure 3. As anticipated, the Mn, Co, Ni, Cu, and Zn KK-edge EXAFS features [Fig. 3(a)] are similar, but distinct from the Cr KK-edge.

Figure 3. Probing the local structure using EXAFS. a The kk weighted EXAFS spectra in A5Cr2O4\mathrm{A}^{5}\mathrm{Cr}_{2}\mathrm{O}_{4}. The Fourier transform of the EXAFS spectra at b Cr KK-edge and c AA KK-edges in the parent oxides and A5Cr2O4\mathrm{A}^{5}\mathrm{Cr}_{2}\mathrm{O}_{4}. Inset panels show the first and second nearest neighbor distances (b) for Cr, (c) for AA site.

The Fourier transform (FT) of k2⋅χ(k)k^2\cdot\chi(k) of Cr and AA KK-edges for each of the parent compounds and A5Cr2O4A^{5}\mathrm{Cr}_2\mathrm{O}_4 are shown in Figure 3(b) and (c), respectively. The first peak at 1.55 Å in both Cr and AA KK-edge data suggests similar Cr-O and AA-O distances. The second peak at 2.5 Å in Cr KK-edge data corresponds to Cr-Cr distance, while the one at 3 Å in AA KK-edge data corresponds to AA-Cr distance, implying different cation environments around Cr and the AA cations. We also note that the real scattering distance shifts by approximately 0.5 Å as the phase shift in the Fourier transform remains uncorrected.

The FT of k2⋅χ(k)k^2\cdot\chi(k) for Cr KK in A5Cr2O4A^{5}\mathrm{Cr}_2\mathrm{O}_4 [Fig. 3(b)] shows similar features like the parent compounds (except CuCr2O4\mathrm{CuCr}_2\mathrm{O}_4). However, Figure 3(c) reveals significant changes in local structures around Cu and Mn in A5Cr2O4A^{5}\mathrm{Cr}_2\mathrm{O}_4 compared to CuCr2O4\mathrm{CuCr}_2\mathrm{O}_4 and MnCr2O4\mathrm{MnCr}_2\mathrm{O}_4, respectively. This is likely due to the difference in crystal symmetry (cubic vs. tetragonal) and lattice volume changes. Local structures around Co, Ni, and Zn in A5Cr2O4A^{5}\mathrm{Cr}_2\mathrm{O}_4 are similar to their parent compounds, except for a slight change in Zn-Cr distance. To quantify all differences in local structures, we performed fittings for the Cr KK edge and AA KK-edge (A=MnA = \mathrm{Mn}, Co, Ni, Cu and Zn) spectra, as discussed below.

Local structure around Cr: For the Cr KK-edge EXAFS, we employed a kk range of 2 to 12 Å−1^{-1} and an RR range of 1 to 3.7 Å for the fittings (see Figure 4(a), Fig. S4, and tbl:S2-S4 in the Supplementary). All analyses were performed considering the structure symmetries determined by XRD: tetragonal for CuCr2O4\mathrm{CuCr}_2\mathrm{O}_4 and NiCr2O4\mathrm{NiCr}_2\mathrm{O}_4, and cubic for the remaining parent compounds and A5Cr2O4A^{5}\mathrm{Cr}_2\mathrm{O}_4. In the cubic model, the Cr site has 6 O as the first neighbor, 6 Cr as the second neighbor, and 6 AA cations as the third neighbor. The bond lengths obtained from the EXAFS fittings have been shown in Figure 4(b)-(Figure 4d), respectively. In the tetragonal structure, the six equivalent bond lengths split into two distinct groups: four with one distance and two with another. Therefore, for NiCr2O4\mathrm{NiCr}_2\mathrm{O}_4 and CuCr2O4\mathrm{CuCr}_2\mathrm{O}_4, the weighted average (denoted by closed circles) is also plotted for easier comparison in Figure 4(b)-(Figure 4d). From the analysis, we could infer that the bond distances Cr-O (1.97 Å), Cr-Cr (2.96 Å) and Cr-AA (3.46 Å) in A5Cr2O4A^{5}\mathrm{Cr}_2\mathrm{O}_4 are akin to that of CoCr2O4\mathrm{CoCr}_2\mathrm{O}_4, ZnCr2O4\mathrm{ZnCr}_2\mathrm{O}_4 and also with the weighted average bond lengths of NiCr2O4\mathrm{NiCr}_2\mathrm{O}_4. Consistent

Figure 4. Analysis of local structure in the octahedral environment. a The Fourier transformed EXAFS spectrum along with the fitted data [the magnitude ∣χ(R)∣\lvert\chi(R)\rvert and the real part Re.⁡χ(R)\operatorname{Re.}\chi(R)] in 5ACr2O4^{5}\mathrm{A}\mathrm{Cr}_{2}\mathrm{O}_{4}. The bond distances from Cr for b first neighbor O, c second neighbor Cr and d third neighbor A ions as obtained from EXAFS fittings for every pristine chromite spinels and 5ACr2O4^{5}\mathrm{A}\mathrm{Cr}_{2}\mathrm{O}_{4}. Due to Jahn-Teller distortion, NiCr2O4\mathrm{NiCr}_{2}\mathrm{O}_{4} and CuCr2O4\mathrm{CuCr}_{2}\mathrm{O}_{4} display two bond lengths (drawn as open circles), whose weighted average (denoted by the closed circle) is also plotted for ease of comparison. Histogram plots for e Cr-O, and f Cr-Cr bond lengths, obtained from DFT calculations of 10 different disordered structures.

with the difference in lattice constant, these bond lengths are higher in MnCr2O4\mathrm{MnCr}_{2}\mathrm{O}_{4}. In addition, the average Cr-O and Cr-AA bond distances of CuCr2O4\mathrm{CuCr}_{2}\mathrm{O}_{4} are lower than A5Cr2O4\mathrm{A}^{5}\mathrm{Cr}_{2}\mathrm{O}_{4}. Since CuCr2O4\mathrm{CuCr}_{2}\mathrm{O}_{4} and NiCr2O4\mathrm{NiCr}_{2}\mathrm{O}_{4} exhibit tetragonal structures at 300 K, we attempted to analyze the Cr K-edge EXAFS of A5Cr2O4\mathrm{A}^{5}\mathrm{Cr}_{2}\mathrm{O}_{4} using tetragonal symmetry. However, this yielded unphysical fitting parameters (Table S6, Supplementary), signifying the absence of local Jahn-Teller distortions around Cr.

To further examine any local Jahn-Teller like distortions around Cr, we performed DFT calculations on 10 supercells, each containing 448 atoms. These supercells were generated by randomly distributing 12 Mn, 13 Co, 13 Ni, 13 Cu, and 13 Zn atoms across the 64 AA-sites, creating 10 distinct disordered structures (calculation details are in the Methods section). Histograms of Cr-O and Cr-Cr bond distances, derived from these calculations, are shown in Figure 4(e) and (f), respectively. While a narrow distribution of Cr-O bond distances (∼2.0±0.02\sim2.0 \pm0.02 Å) was observed, no Jahn-Teller distortions were found (our DFT calculations accurately capture Jahn-Teller distortions in CuCr2O4\mathrm{CuCr}_{2}\mathrm{O}_{4}, as shown in Supplementary Table S7). The Cr-Cr bond distances also exhibit a distribution, with the peak position [Figure 4(f)] closely matching the EXAFS-derived value for A5Cr2O4\mathrm{A}^{5}\mathrm{Cr}_{2}\mathrm{O}_{4} [Figure 4(c)]. However, EXAFS is limited in revealing precise distributional information due to its averaging of local environments around all Cr ions.

Local structure around AA sites: To probe the local distortions around AA-sites, we performed fittings for the AA KK-edge spectra (AA = Mn, Co, Ni, Cu and Zn) in every parent compound and A5Cr2O4\mathrm{A}^{5}\mathrm{Cr}_{2}\mathrm{O}_{4} in the kk range of 2 to 14 Å−1^{-1} and the RR range of 1 to 4.5 Å (details are in the Methods section, see Figure 5(a) in main text, Fig. S4 and Supplementary Table S2-S4). Based on XRD results, either cubic or tetragonal symmetry was used for these fittings and all coordination numbers were also kept fixed. Fits with variable coordination numbers (see Supplementary section S2.3 and Table S5) corroborate the reliability of our fixed coordination number approach.

Figure 5. **Analysis of local structure in the tetrahedral environment.**The magnitude of the Fourier transformed EXAFS spectra along with fittings obtained at the a Cu KK-edge in CuCr2O4\mathrm{CuCr}_{2}\mathrm{O}_{4} and A5Cr2O4\mathrm{A}^{5}\mathrm{Cr}_{2}\mathrm{O}_{4}. The bond lengths depicted in [b-c] are obtained from EXAFS fittings for every pristine chromite spinels and A5Cr2O4\mathrm{A}^{5}\mathrm{Cr}_{2}\mathrm{O}_{4}. In c, due to Jahn-Teller distortion, NiCr2O4\mathrm{NiCr}_{2}\mathrm{O}_{4}, and CuCr2O4\mathrm{CuCr}_{2}\mathrm{O}_{4} display two bond lengths between AA and Cr cations (drawn as open circles), whose weighted average (closed circle) is plotted for ease of comparison. Histogram plots for d first neighbor AA-O, and e second neighbor AA-Cr bond lengths, found from DFT calculations of 10 different disordered structures.

We first focus on the parent compounds. For the cubic MnCr2O4\mathrm{MnCr}_{2}\mathrm{O}_{4}, EXAFS analysis indicates that Mn is coordinated with 4 O atoms at 1.99 Å, 12 O atoms at 3.32 Å, 12 Cr atoms at 3.50 Å, and 4 Mn atoms at 3.64 Å. Notably, the Mn-O bond distance, identified as the third neighbor by XRD, was found to be shorter than the Mn-Cr bond distance (second neighbor) in EXAFS fitting. We observe this trend across all six compounds, as well as in previous EXAFS studies [52, 53]. This deviation in bond distances is likely due to the weak scattering contribution from O as a third neighbor, a consequence of its low atomic number. Therefore, the subsequent sections of this paper will primarily focus on the first-neighbor AA-O and second-neighbor AA-Cr distances. It should be noted that the AA-Cr distances are equivalent to the Cr-AA distances, which were independently determined from Cr KK-edge EXAFS fitting. For tetragonal CuCr2O4\mathrm{CuCr}_{2}\mathrm{O}_{4}, EXAFS analysis shows the Cu atom coordinated with 4 O at 1.95 Å in the first shell, 8 Cr at 3.52 Å, and 4 Cr at 3.26 Å in the second shell.

The EXAFS fittings of each AA-site of A5Cr2O4\mathrm{A}^{5}\mathrm{Cr}_{2}\mathrm{O}_{4} were performed considering cubic symmetry in accordance with the XRD result. Excellent fitting has been found for each case, including Cu KK-edge [Figure 5 (a)] and Ni KK-edge (see Supplementary Fig. S3 (c)). We have also attempted to fit Cu KK EXAFS of A5Cr2O4\mathrm{A}^{5}\mathrm{Cr}_{2}\mathrm{O}_{4} using tetragonal symmetry, similar to the parent compound CuCr2O4\mathrm{CuCr}_{2}\mathrm{O}_{4}. However, such fitting results in unphysical parameters (see Supplementary section S2.4, Table S6), indicating the absence of tetragonal distortion, even locally. The comparison of each neighbor distance among the pristine members and doped compound reveals several interesting trends (Figure 5 (b) and (d)). The Mn-O distance in MnCr2O4\mathrm{MnCr}_{2}\mathrm{O}_{4} is the largest, attributed to its larger unit cell volume compared to other pristine materials. Notably, the first neighbor A-O distance of A5Cr2O4\mathrm{A}^{5}\mathrm{Cr}_{2}\mathrm{O}_{4} depends on the specific element positioned at the A-site. The Co-O, Ni-O, and Cu-O distances are very similar, whereas Mn-O and Zn-O distances differ. Also, all the A-O bond distances are smaller than those in the corresponding parent ACr2O4\mathrm{ACr}_{2}\mathrm{O}_{4}, indicating that these local variations are not simply due to changes in the overall crystal volume. Furthermore, second neighbor A-Cr distances [Figure 5(c)], determined from A-site EXAFS in A5Cr2O4\mathrm{A}^{5}\mathrm{Cr}_{2}\mathrm{O}_{4}, vary mildly with the specific A cation.

Next, we discuss the bond lengths at the AA site in A5Cr2O4\mathrm{A}^{5}\mathrm{Cr}_{2}\mathrm{O}_{4} based on DFT calculations. The histogram plots for the first neighbor AA-O distances and the second neighbor AA-Cr distances are presented in Figure 5 (d) and (e), respectively. Despite considering ten different disordered structures in our calculations, the distances for Mn-O, Co-O, Ni-O, and Zn-O do not show any statistical distribution, suggesting well-defined bond lengths. In contrast, the Cu-O bond distances display a broad range of values. Notably, the trends observed for the AA-O bond distances closely align with our EXAFS results, with Mn-O being the longest and Zn-O the shortest. Interestingly, the second neighbor distances for Mn-Cr, Co-Cr, Ni-Cr, and Zn-Cr also show a distribution, as illustrated in Figure 5 (e). The peak positions of these distributions are similar to the Cr-A distances obtained from EXAFS, shown in Figure 5 (c). Furthermore, the distribution width for Cu-Cr bonds is significantly broader compared to the other AA-Cr bonds. This finding corroborates our EXAFS analysis, which revealed a higher σ2\sigma^{2} (mean squared variation of bond length) for Cu-O and Cu-Cr distances compared to other AA-O and AA-Cr bonds ( see Supplementary Fig. S5).

Accommodation of local distortions: Our EXAFS and DFT analyses demonstrate that element-specific structural distortions in A5Cr2O4\mathrm{A}^{5}\mathrm{Cr}_{2}\mathrm{O}_{4} extend beyond the first coordination shell of the AA sites. Notably, the broad distribution of Cu-O bond distances, alongside specific values for other AA-O distances, highlights the crucial role of the highly flexible CuO4\mathrm{CuO}_{4} tetrahedral units in accommodating these local distortions. Consequently, this flexibility influences other bond distances: the connection between CuO4\mathrm{CuO}_{4} and CrO6\mathrm{CrO}_{6} unit via a common oxygen (inset of Figure 3(c)) leads to a broad Cu-Cr distance distribution, while Cr-O and Cr-Cr distances show narrower distributions without Jahn-Teller distortion. Additionally, the connectivity of each CrO6\mathrm{CrO}_{6} octahedron to five AO4A\mathrm{O}_{4} units (AA = Mn, Co, Ni, Cu, Zn) contributes to the narrower distributions of other Cr-AA bond lengths.

Correlation between structural distortions and magnetic interaction: These bond lengths are expected to play a crucial role in comprehending the strength of magnetic interactions in ACr2O4A\mathrm{Cr}_{2}\mathrm{O}_{4} spinels. The theory of ground state magnetic configuration of cubic AB2O4A B_{2}\mathrm{O}_{4} is very often described by the following Hamiltonian with classical Heisenberg spins considering BB-BB, and AA-BB exchanges, initially proposed by Lyons, Kaplan, Dwight, and Menyuk [38, 54, 55].

H=2JABSASB(∑⟨ij⟩A,Bσ⃗iA⋅σ⃗jB+3u4∑⟨ij⟩B,Bσ⃗iB⋅σ⃗jB)(1)H = 2J_{AB}S_AS_B\left(\sum_{\langle ij\rangle}^{A,B}\vec{\sigma}^{A}_{i}\cdot\vec{\sigma}^{B}_{j}+\frac{3u}{4}\sum_{\langle ij\rangle}^{B,B}\vec{\sigma}^{B}_{i}\cdot\vec{\sigma}^{B}_{j}\right) \tag*{(1)}

The sums are over nearest-neighbor AA-BB and BB-BB pairs and the parameter u=4JBBSB3JABSAu=\frac{4J_{BB}S_B}{3J_{AB}S_A} and σ⃗jα=S⃗jα/Sα\vec{\sigma}^{\alpha}_{j}=\vec{S}^{\alpha}_{j}/S^{\alpha} with α=A\alpha=A and BB. The interaction within the diamond sublattice (JAAJ_{AA}) has also been claimed to be important in recent studies [56, 57]. In chromite spinels, the magnetic interaction between two Cr is a direct exchange and thus depends strongly on the Cr-Cr distance [56]. The superexchange between AA and Cr is mediated through interconnecting oxygen, and the strength will depend on the bond lengths AA-O and Cr-O, AA-O-Cr bond angle, and the electronic configuration of AA site ions. Surprisingly, the θCW\theta_{\mathrm{CW}}, which is a measure of molecular field and considered as an approximate indicator of the strength of mean-field magnetic interaction between the ions [58], directly correlates with the Cr-Cr distance [39]. Thus, we have focused on finding out the relation between θCW\theta_{\mathrm{CW}} and the bond lengths at 300 K obtained from the EXAFS analysis.

The temperature-dependent magnetic susceptibility [χ=M/H\chi=M/H] for A5^{5}Cr2_2O4_4, measured under a magnetic field (HH) of 5000 Oe in field cooled condition has been depicted as an inset of Figure 6 (a). We found a magnetic transition around 41 K. The main panel represents the fitting of the inverse of dc susceptibility at high temperature using molecular field theory of a ferrimagnet [59]

Figure 6. a Fitting of inverse magnetic dc susceptibility using Curie-Weiss equation above TNT_{\mathrm{N}} in A5Cr2O4A^{5}\mathrm{Cr}_{2}\mathrm{O}_{4} at 5000 Oe. Inset features field cooled (FC) dc susceptibility as a function of temperature. −θCW-\theta_{\mathrm{CW}} is plotted as a function of b Cr-Cr bond distance and AA-site spin and c Cr-O bond distance and AA site spin in parent oxides and A5Cr2O4A^{5}\mathrm{Cr}_{2}\mathrm{O}_{4}. d A comparision of the magnetic exchange interaction energy between two Cr cations (JCrCrJ_{\mathrm{CrCr}}), between Cr and AA (JACrJ_{\mathrm{ACr}}), and between two AA cations (JAAJ_{\mathrm{AA}}) in MnCr2O4\mathrm{MnCr}_{2}\mathrm{O}_{4} and A5Cr2O4A^{5}\mathrm{Cr}_{2}\mathrm{O}_{4}.

χ−1=T−θCWCA+2CB−C′′T−θ′(2)\chi^{-1}=\frac{T-\theta_{\mathrm{CW}}}{C_A+2C_B}-\frac{C''}{T-\theta'} \tag*{(2)}

The first term is the hyperbolic high-temperature linear part with a Curie-Weiss form, where CAC_A and CBC_B correspond to Curie constants related to the two magnetic sublattices MAM_A and MBM_B, respectively. θCW\theta_{\mathrm{CW}} is the Curie-Weiss temperature. The second term is the hyperbolic low-TT asymptote, where C′′C'' and θ′\theta' are constants akin to different Weiss coefficients that represent the inter and intrasublattice interactions. From this fitting, we have obtained a Curie-Weiss temperature of θCW=−432\theta_{\mathrm{CW}}=-432 K and the effective magnetic moment of 6.33 μB\mu_B/f.u. using the formula μeff=3KB(CA+2CB)NA\mu_{\mathrm{eff}}=\sqrt{\frac{3K_B(C_A+2C_B)}{N_A}} [60], where KBK_B is Boltzmann’s constant and NAN_A is Avogadro’s number. Interestingly, μeff\mu_{\mathrm{eff}} is very similar to the expected value of 6.26 μB\mu_B/f.u., calculated by considering the average magnetic moments of A2+A^{2+} (A=A= Mn, Co, Ni, Cu; Zn2+^{2+} is nonmagnetic) and Cr3+^{3+} of A5^{5}Cr2_2O4_4 (μeff=2μCr2+μA2\mu_{\mathrm{eff}}=\sqrt{2\mu_{\mathrm{Cr}}^2+\mu_A^2}). The most surprising finding is that despite having a series of magnetic interactions [Cr-AA and AA-A′A' with AA, A′=A'= Mn, Co, Ni, Cu], the θCW\theta_{\mathrm{CW}} of A5^{5}Cr2_2O4_4 is comparable to NiCr2_2O4_4 [44] (also see Supplementary Figure S6) and MnCr2_2O4_4 [56]. The effective magnetic moment also closely resembles NiCr2_2O4_4 (6.64 μB6.64\,\mu_B/f.u.). These findings also indicate that the net magnetic interaction, felt by a magnetic ion in CCO, can be treated using a mean-field approach.

To understand the effect of local distortions on magnetism, ∣θCW∣|\theta_{\mathrm{CW}}| for all six compounds have been plotted as a function of EXAFS derived bond lengths and the AA-site spin value in Figure 6(b), (Figure 6c). The θCW\theta_{\mathrm{CW}} of the parent compounds AACr2_2O4_4 is obtained from Ref. [44, 56, 61] and an average of AA-site spin (SA=1.1S_A=1.1) for A5A^5Cr2_2O4_4 has been considered for these plots. The Cr-Cr bond length (Figure 6 (b)) is considered as it corresponds to the Cr-Cr direct exchange. The Cr-O bond length is also plotted in connection with the AA-O-Cr superexchange path (Figure 6 (b)). While the AA-O bond length also plays a role in AA-O-Cr superexchange strength, we were unable to create a similar plot for AA-O bond lengths because this distance depends on the specific atom occupying the AA-site in A5A^5Cr2_2O4_4. The θCW\theta_{\mathrm{CW}} of A5A^5Cr2_2O4_4 is closer to the value of NiCr2_2O4_4 and MnCr2_2O4_4. We have further evaluated the mean-field magnetic exchange parameters from our magnetization data, following the process described in Ref. [56] [also see Supplementary section S4]. The exchange interaction parameters JBBJ_{BB} (interactions between two Cr3+^{3+}), JABJ_{AB} (between A2+A^{2+} and Cr3+^{3+}), and JAAJ_{AA} (between two A2+A^{2+} cations) have been compared in Figure 6(d). The exchange parameters for MnCr2_2O4_4 have been adapted from Ref. [56]. Interestingly, the JBBJ_{BB} interaction shows almost no difference between these compounds. However, the JABJ_{AB} and JAAJ_{AA} values for A5A^5Cr2_2O4_4 are higher than those of MnCr2_2O4_4. The extraction of these JJs using equation (2) is not possible for NiCr2_2O4_4 due to an anomaly in the magnetic susceptibility at the cubic-to-tetragonal transition (∼315\sim315 K, see Supplementary Fig S6). However, Figure 6 (b) and (Figure 6c) clearly demonstrate the close similarity between A5A^5Cr2_2O4_4 and NiCr2_2O4_4 in terms of key parameters like Cr-Cr distance, Cr-O distance, and AA-site spin and θCW\theta_{\mathrm{CW}}. This strong resemblance highlights the crucial role of local bond lengths around the Cr ions in determining the mean-field magnetic interactions within A5A^5Cr2_2O4_4.

Our DFT calculations also show that the local Cr moment increases with Cr-Cr and Cr-A distances (see Supplementary Figure S7). This indicates that the moments become more localized as they are placed further away. A more rigorous analysis of the connection between structure and magnetism may be obtained from the variation of the magnetic exchange parameters [62]. The extraction of pairwise exchange parameters for such a complicated disordered system is a highly non-trivial task and will be attempted to be done in the near future.

Conclusions

We have synthesized a compositionally complex spinel oxide A5Cr2O4A^{5}\mathrm{Cr}_{2}\mathrm{O}_{4}, with Cr3+\mathrm{Cr}^{3+} ions occupying the octahedral site and a uniform distribution of A2+A^{2+} (A=Mn,Co,Ni,CuA = \mathrm{Mn}, \mathrm{Co}, \mathrm{Ni}, \mathrm{Cu}, and Zn\mathrm{Zn}) ions in the tetrahedral site. Our investigation of the local structure employing element-specific EXAFS analysis and DFT calculations with various disordered configurations reveals several unique features that distinguish it from previously reported high entropy oxides. Unlike HEOs with rock-salt structures [34, 63], where local Jahn-Teller distortions around Cu2+\mathrm{Cu}^{2+} ions are typically preserved, our study reveals a complete absence of such distortions in A5Cr2O4A^{5}\mathrm{Cr}_{2}\mathrm{O}_{4}. In contrast to other HEOs, where local distortions are limited to the first nearest neighbors of the doped cations [34, 35], in the present study, A5Cr2O4A^{5}\mathrm{Cr}_{2}\mathrm{O}_{4} exhibits variation in local distortions extending beyond the first neighbors. Despite a broad distribution of Cu-O bond distances, other AA-O distances acquire specific values, implying the high flexibility of CuO4\mathrm{CuO}_{4} tetrahedral units to maintain an overall cubic structure by adjusting their positions. Such adjustment also leads to a broad distribution of second neighboring Cu-Cr distances and a narrow distribution of other AA-Cr, Cr-Cr and Cr-O bond lengths. Despite substantial local distortions, the mean-field magnetic interaction energies of A5Cr2O4A^{5}\mathrm{Cr}_{2}\mathrm{O}_{4} are remarkably similar to those of NiCr2O4\mathrm{NiCr}_{2}\mathrm{O}_{4} due to their closely matched average AA-site spin value, as well as their average Cr-O and Cr-Cr bond lengths.

Unveiling the temperature dependence of A5Cr2O4A^{5}\mathrm{Cr}_{2}\mathrm{O}_{4}’s long-range and local structures presents a compelling avenue for future research as some of the constituent members undergo structural transitions below room temperature [44]. Future investigations into the spin arrangements and potential multiferroic phases are warranted. Furthermore, we believe that our approach, which compares EXAFS analysis of CCO with the constituent parent members along with the DFT calculations for a set of disordered configurations, would be a powerful tool for revealing subtle details regarding structural modifications in other compositionally complex materials.

Methods

Synthesis: Polycrystalline samples of five parent compounds ACr2O4A\mathrm{Cr}_{2}\mathrm{O}_{4} (A=Mn,Co,Ni,CuA = \mathrm{Mn}, \mathrm{Co}, \mathrm{Ni}, \mathrm{Cu} and Zn\mathrm{Zn}) were synthesized by conventional solid-state synthesis with a stoichiometric amount of Cr2O3\mathrm{Cr}_{2}\mathrm{O}_{3} and AOAO. The first heating was carried out at 900∘C900^{\circ}\mathrm{C}, followed by a second heat treatment at 1300∘C1300^{\circ}\mathrm{C} with intermediate grindings. The annealing of MnCr2O4\mathrm{MnCr}_{2}\mathrm{O}_{4} and CuCr2O4\mathrm{CuCr}_{2}\mathrm{O}_{4} were performed in argon and oxygen atmosphere, respectively, while the rest of the compounds were heated in air. The A5Cr2O4A^{5}\mathrm{Cr}_{2}\mathrm{O}_{4} was synthesized in a similar route in the air.

Experimental details: All the experiments were carried out at ambient temperatures. The sample purity of all samples was checked by powder XRD using a laboratory-based Rigaku Smartlab diffractometer. The final XRD patterns were further refined by the Rietveld method using the FULLPROF suite [64]. The Raman spectra were recorded using Confocal Photoluminescence Raman Spectro Microscope. Data was collected using 532 nm LASER and 1800 rules/mm grating in 100–800 cm−1\mathrm{cm}^{-1} wavenumber range. The temperature-dependent magnetization measurement was carried out in the range of 5 K to 400 K using a commercial SQUID-VSM MPMS from M/s Quantum Design, USA.

XAS spectra for L3,2L_{3,2} edges of Cr, Mn, Co, Ni, Cu of the A5Cr2O4A^{5}\mathrm{Cr}_{2}\mathrm{O}_{4} were recorded in total electron yield mode at the beamline 4.0.2 of the Advanced Light Source, USA. Ni L3,2L_{3,2} edge of NiCr2_2O4_4 and Cu L3,2L_{3,2} edge of CuCr2_2O4_4 were also measured.

EXAFS measurements for all transition metal KK-edge for all five parent compounds and A5Cr2O4A^{5}\mathrm{Cr}_{2}\mathrm{O}_{4} have been performed at the P65 beamline, PETRA III Synchrotron Source (DESY, Hamburg, Germany) and at beamline 20-BM of the Advanced Photon Source, USA. For these transmission mode experiments, the absorbers were prepared by uniformly coating fine powders on scotch tape. The incident and transmitted photon energies were recorded simultaneously using gas ionization chambers as detectors. For each KK edge, at least three scans were taken to average the statistical noise. All EXAFS data presented in this manuscript were acquired during the same beamtime at the P65 beamline. Therefore, the experimental setup was identical for all parent ACr2_2O4_4 and A5Cr2O4A^{5}\mathrm{Cr}_{2}\mathrm{O}_{4} samples.

EXAFS analysis details: The analysis was conducted using well-established procedures from the DEMETER Suite [65]. The spectra for each transition metal edge were calibrated with the corresponding standard metal foils. In pristine ACr2_2O4_4 oxides, we performed fittings for the A K-edge spectra (AA = Mn, Co, Ni, Cu, and Zn), using a kk range of 2 to 14 A˚−1\AA^{-1} and RR range of 1 to 4.5 A˚\AA. For the Cr KK-edge, we employed a kk range of 2 to 12 A˚−1\AA^{-1} and an RR range of 1 to 3.7 A˚\AA for the fittings. To prevent interference from the adjacent absorption edge in A5Cr2O4A^{5}\mathrm{Cr}_{2}\mathrm{O}_{4}, we truncated the spectra above 12 A˚−1\AA^{-1} in kk-space. The fittings were performed in the kk range of 2 to 11 A˚−1\AA^{-1} and RR range of 1 to 3.7 A˚\AA in all six edges (see Figure 4(a), Figure 5(a), Fig. S3, and Tables S2-S4 in the Supplementary Materials). In our fitting process, we primarily considered the following parameters: coordination number (NN), amplitude reduction factor (S02S_{0}^{2}), energy shift (E0)(E_0), the change in bond length (ΔR)(\Delta R), and the mean squared displacement (σ2)(\sigma^2), also known as the Debye factor.

For the AA KK edge fitting in cubic ACr2O4\mathrm{ACr_2O_4} (A=Mn,Co,ZnA = \mathrm{Mn, Co, Zn}), we utilized four paths associated with the direct scattering: the first neighbor A-O, the second neighbor A-Cr, the third neighbor A-O, and the fourth neighbor A-A. The parameters S02S_0^2 and E0E_0 were taken as variables for the fitting. ΔR\Delta R and σ2\sigma^2 were varied for each path considered. As a result, we had four values for ΔR\Delta R, four values for σ2\sigma^2, one value for S02S_0^2, and one value for E0E_0, totaling ten parameters. For the Cr KK fitting, we focused on three coordination shells: Cr-O, Cr-Cr, and Cr-A. Using a similar approach, we employed a total of eight parameters for this fitting. It is important to note that the AA KK and Cr KK fittings were conducted separately, and the parameters used in the two fittings are not correlated.

In CuCr2O4\mathrm{CuCr_2O_4}, at the Cu KK edge, the Jahn-Teller distortion leads to splitting in the second and third coordination shells of Cu-Cr and Cu-O respectively. Hence, two different values for ΔR\Delta R and σ2\sigma^2 were used within a single shell for both of these paths. As a result, six paths involving direct scatterers were used in the fitting, compared to four paths in the cubic phase. This change increased the total number of parameters from ten in the cubic phase to fourteen in the tetragonal phase. For the Cr KK edge, the Jahn-Teller distortion causes splitting in all three coordination shells: Cr-O, Cr-Cr, and Cr-Cu. Here, we used six paths in the fitting, instead of three in the cubic phase, which increased the number of total parameters from eight to fourteen. In the case of NiCr2O4\mathrm{NiCr_2O_4}, the Jahn-Teller splitting is smaller than the EXAFS resolution [ΔR=π/2×(kmax⁡−kmin⁡)][\Delta R = \pi/2 \times(k_{\max} - k_{\min})], which is approximately 0.16 Å. Since XRD indicated a tetragonal phase, we adopted a tetragonal model similar to that of CuCr2O4\mathrm{CuCr_2O_4} to ensure consistency with the XRD results.

The coordination number NN was kept fixed during the analysis. All parent compounds are normal spinels, ruling out any site occupancy disorder between the A (tetrahedral) and Cr (octahedral) site (second neighbors). However, we did try fittings by varying the coordination numbers of the first shell (A-O and Cr-O). Although a small deviation from the stoichiometric value was observed, this deviation was consistent between all the parent compounds and the compositionally complex A5Cr2O4\mathrm{A^5Cr_2O_4} (see section S2.3 and tbl:S5 in Supplementary). Furthermore, the coordination numbers obtained from fitting agree with the stoichiometric values within the statistical error of the fit. Given the excellent agreement between the magnetic properties of our parent compounds and previously published results, we attribute these small deviations in oxygen coordination number to the inherent resolution limitations of EXAFS fitting.

In A5Cr2O4\mathrm{A^5Cr_2O_4}, our XAS measurements and XANES spectra confirm a normal spinel structure. These confirm the presence of all AA (Mn, Co, Ni, Cu, and Zn) cations at the tetrahedral site, similar to all the parent compounds. Therefore, Cr was modeled in octahedral site and the AA ions in tetrahedral site for the EXAFS fitting. For the fitting of the AA-site EXAFS in A5A^{5}Cr2_2O4_4, we chose the S02S_{0}^{2} value determined from the fitting of the corresponding AA-site in the parent compound ACr2_2O4_4. In line with the spinel structure, we considered the following direct scattering paths for the AA KK absorber: first neighbor pair A-O (coordination 4), second neighbor A-Cr (12), third neighbor again A-O (12), and fourth neighbor AA-A (4). In this compound, there is a potential presence of five AA elements (Mn, Co, Ni, Cu, and Zn) in the fourth coordination shell with a total coordination number of 4. For instance, in the Co KK EXAFS, we have the fourth neighbor pairs as Co-Mn, Co-Ni, Co-Cu, Co-Zn, and Co-Co. Hence, in the fittings of every AA KK edge we used all the five pairs as fourth neighbors each with a coordination of 0.8.

In the Cr KK EXAFS fitting of A5A^{5}Cr2_2O4_4, we allowed S02S_{0}^{2} to vary. We used the following direct scattering paths: the first neighbor pair Cr-O (6), the second Cr-Cr (6), and the third Cr-A (6). In this case, the third neighbor, Cr-A, has a coordination number of 6, and five AA elements can be present. Hence, we considered the pairs Cr-Mn, Cr-Co, Cr-Ni, Cr-Cu, and Cr-Zn, each of which with a coordination of 1.2.

In addition, we also checked with various combinations of elements and coordination at the AA site as the fourth neighbor from AA and third neighbor from Cr, finding no significant variations in the bond lengths, reported within the main text.

DFT calculations: A cubic spinel structure of A5A^{5}Cr2_2O4_4 was utilized to generate ten different random oxide supercells of 2×2×22 \times2 \times2 dimensions, consisting of 448 atoms (64 AA, 128 Cr, and 256 O atoms). To form the random distribution, 12 Mn, 13 Co, 13 Ni, 13 Cu, and 13 Zn atoms were distributed among the 64 available AA sites. Each of the ten random oxides was created by randomly rearranging the AA sites while keeping the number of each type of atom constant We conducted structural optimization using the Vienna Ab initio Simulation Package (VASP) based on plane wave basis set and projector augmented wave pseudopotentials [66, 67]. The POSCAR files of the ten different structures have been supplied as a separate file along with the manuscript. The exchange-correlation potential was described using the generalized gradient approximation (GGA) with the Perdew, Burke, and Ernzerhof (PBE) functional [68]. A static Hubbard correction was effectively applied to account for localized Coulomb interactions in highly correlated 3d transition metals, following the Dudarev approach [69]. The UeffU_{\mathrm{eff}} values were set to 4.0, 3.0, 5.0, 8.0, 8.0, and 3.0 eV for Mn, Co, Ni, Cu, Zn, and Cr, respectively, in line with the reported values for transition metal oxides [70, 71, 72, 73]. This setup resulted in a good agreement in bond lengths between experimental data and DFT calculations. For Brillouin zone integration, a Gamma-centered 1×1×11 \times1 \times1 k-point grid was employed. The lattice constants were determined based on experimental results. The equilibrium atomic positions were obtained via energy minimization, employing the conjugate gradient method until the force components on each atom fell below 0.010.01 eV/Å.

Data availability

All data are available from the corresponding authors upon reasonable request,

Acknowledgements

The authors acknowledge the uses of central facilities of the department of Physics, IISc Bangalore, funded by the FIST program of DST (Department of Science and Technology), India. SM acknowledges funding support from a SERB Core Research grant (Grant No. CRG/2022/001906). RN thanks the Indian Institute of Science for support through Sir C. V. Raman postdoctoral fellowship program and Prof. K.R.S. Priolkar for commenting on the manuscript. SD and NB acknowledge funding from the Prime Minister’s Research Fellowship (PMRF), MoE, Government of India. UGC-DAE Consortium for Scientific Research, Kalpakkam Node, Kokilamedu is acknowledged for providing SQUID-VSM MPMS facility for conducting magnetic measurements, which is part of this work. Portions of this research were carried out at the light source PETRA III DESY, a member of the Helmholtz Association (HGF). Financial support by the Department of Science & Technology (Government of India) provided within the framework of the India@DESY collaboration is gratefully acknowledged. This research used resources of the Advanced Photon Source, a U.S. Department of Energy Office of Science User Facility operated by Argonne National Laboratory under Contract No. DE-AC02-06CH11357. This research used resources of the Advanced Light Source, which is a Department of Energy Office of Science User Facility under Contract No. DE-AC02-05CH11231. B.S. acknowledges financial support from Swedish Research Council (grant no. 2022-04309) and STINT Mobility Grant for Internationalization (grant no. MG2022-9386). The computations were enabled by resources provided by the National Academic Infrastructure for Supercomputing in Sweden (NAISS) at UPPMAX (NAISS 2024/5-258) and at NSC and PDC (NAISS 2023/3-42) partially funded by the Swedish Research Council through grant agreement no. 2022-06725. B.S. also acknowledges the allocation of supercomputing hours granted by the EuroHPC JU Development Access call in LUMI-C supercomputer (grant no. EHPC-DEV-2024D04-071) in Finland. S.E. acknowledges the allocation of supercomputing hours granted by the EuroHPC JU Development Access call in LUMI-C supercomputer (grant no. EHPC-DEV-2024D03-043) in Finland and Karolina supercomputer (grant no. EU2023D11-039) in Czech Republic.

Author contribution

SM conceived and supervised the project. RN and SD synthesized, characterized the samples and analyzed all results. RN, SD, NB, CK carried out soft X-ray absorption spectroscopy measurements. RN, NB, TD, GES performed EXAFS experiments. S.E. has performed all the calculations based on DFT, and B.S. has supervised the theoretical part. RN and SM wrote the manuscript. All authors discussed the results and commented on the manuscript.

Competing interests

The authors declare no competing interests.

References

  1. [1]George, E. P., Raabe, D. & Ritchie, R. O. High-entropy alloys. Nature reviews materials 4, 515–534 (2019).
  2. [2]Sarkar, A. et al. High-entropy oxides: fundamental aspects and electrochemical properties. Advanced materials 31, 1806236 (2019).DOI
  3. [3]Oses, C., Toher, C. & Curtarolo, S. High-entropy ceramics. Nature Reviews Materials 5, 295–309 (2020).DOI
  4. [4]Musicó, B. L. et al. The emergent field of high entropy oxides: Design, prospects, challenges, and opportunities for tailoring material properties. APL Materials 8, 040912 (2020). URL https://doi.org/10.1063/5.0003149. https://pubs.aip.org/aip/apm/article-pdf/doi/10.1063/5.0003149/14563544/040912_1_online.pdf.
  5. [5]Brahlek, M. et al. What is in a name: Defining “high entropy” oxides. APL Materials 10, 110902 (2022). URL https://doi.org/10.1063/5.0122727. https://pubs.aip.org/aip/apm/article-pdf/doi/10.1063/5.0122727/16490715/110902_1-online.pdf.
  6. [6]Kotsonis, G. N. et al. High-entropy oxides: Harnessing crystalline disorder for emergent functionality. Journal of the American Ceramic Society 106, 5587–5611 (2023).DOI
  7. [7]Mazza, A. R. et al. Embracing disorder in quantum materials design. Applied Physics Letters 124, 230501 (2024). URL https://doi.org/10.1063/5.0203647. https://pubs.aip.org/aip/apl/article-pdf/doi/10.1063/5.0203647/19978559/230501_1_5.0203647.pdf.
  8. [8]Cantor, B., Chang, I., Knight, P. & Vincent, A. Microstructural development in equiatomic multicomponent alloys. Materials Science and Engineering: A 375, 213–218 (2004).DOI
  9. [9]Yeh, J.-W. et al. Nanostructured high-entropy alloys with multiple principal elements: novel alloy design concepts and outcomes. Advanced engineering materials 6, 299–303 (2004).
  10. [10]Rost, C. M. et al. Entropy-stabilized oxides. Nature communications 6, 8485 (2015).
  11. [11]Djenadic, R. et al. Multicomponent equiatomic rare earth oxides. Materials Research Letters 5, 102–109 (2017).
  12. [12]Jiang, S. et al. A new class of high-entropy perovskite oxides. Scripta Materialia 142, 116–120 (2018).DOI
  13. [13]Sharma, Y. et al. Single-crystal high entropy perovskite oxide epitaxial films. Physical Review Materials 2, 060404 (2018).DOI
  14. [14]Patel, R. K. et al. Epitaxial stabilization of ultra thin films of high entropy perovskite. Applied Physics Letters 116, 071601 (2020).DOI
  15. [15]Brahlek, M. et al. Unexpected crystalline homogeneity from the disordered bond network in La(Cr₀.₂Mn₀.₂Fe₀.₂Co₀.₂Ni₀.₂)O₃ films. Phys. Rev. Mater. 4, 054407 (2020). URL https://link.aps.org/doi/10.1103/PhysRevMaterials.4.054407.DOI
  16. [16]Musicó, B. et al. Tunable magnetic ordering through cation selection in entropic spinel oxides. Phys. Rev. Mater. 3, 104416 (2019). URL https://link.aps.org/doi/10.1103/PhysRevMaterials.3.104416.DOI
  17. [17]Sharma, Y. et al. Magnetic texture in insulating single crystal high entropy oxide spinel films. ACS applied materials & interfaces 13, 17971–17977 (2021).arxiv.org/abs/2103.16722
  18. [18]Johnstone, G. H. et al. Entropy engineering and tunable magnetic order in the spinel high-entropy oxide. Journal of the American Chemical Society 144, 20590–20600 (2022).DOI
  19. [19]Wright, A. J. et al. Size disorder as a descriptor for predicting reduced thermal conductivity in medium-and high-entropy pyrochlore oxides. Scripta Materialia 181, 76–81 (2020).arxiv.org/abs/1912.11734
  20. [20]Jiang, B. et al. Probing the local site disorder and distortion in pyrochlore high-entropy oxides. Journal of the American Chemical Society 143, 4193–4204 (2020).DOI
  21. [21]Kinsler-Fedon, C. et al. Synthesis, characterization, and single-crystal growth of a high-entropy rare-earth pyrochlore oxide. Phys. Rev. Mater. 4, 104411 (2020). URL https://link.aps.org/doi/10.1103/PhysRevMaterials.4.104411.
  22. [22]Sarkar, A. et al. High entropy oxides for reversible energy storage. Nature communications 9, 3400 (2018).DOI
  23. [23]Chen, H. et al. Entropy-stabilized metal oxide solid solutions as co oxidation catalysts with high-temperature stability. Journal of Materials Chemistry A 6, 11129–11133 (2018).DOI
  24. [24]Braun, J. L. et al. Charge-induced disorder controls the thermal conductivity of entropy-stabilized oxides. Advanced materials 30, 1805004 (2018).DOI
  25. [25]Kante, M. V. et al. A high entropy oxide as high-activity electrocatalyst for water oxidation. ACS Nano 17, 5329 (2023). URL https://pubs.acs.org/doi/10.1021/acsnano.2c08096.DOI
  26. [26]Patel, R. K. et al. Thickness dependent OER electrocatalysis of epitaxial thin film of high entropy oxide. Applied Physics Reviews 10, 031407 (2023). URL https://doi.org/10.1063/5.0146005. https://pubs.aip.org/aip/apr/article-pdf/doi/10.1063/5.0146005/18068792/031407_1_5.0146005.pdf.
  27. [27]Zhao, B. et al. High-entropy enhanced microwave attenuation in titanate perovskites. Advanced Materials 35, 2210243 (2023).DOI
  28. [28]Schweidler, S. et al. High-entropy materials for energy and electronic applications. Nature Reviews Materials 1–16 (2024).
  29. [29]Moniri, S. et al. Three-dimensional atomic structure and local chemical order of medium-and high-entropy nanoalloys. Nature 624, 564–569 (2023).DOI
  30. [30]Aamlid, S. S., Oudah, M., Rottler, J. & Hallas, A. M. Understanding the role of entropy in high entropy oxides. Journal of the American Chemical Society 145, 5991–6006 (2023).DOI
  31. [31]Ruffoni, M., Pettifer, R., Pascarelli, S., Trapananti, A. & Mathon, O. Probing atomic displacements with thermal differential exafs. Journal of Synchrotron Radiation 14, 421–425 (2007).pubmed.ncbi.nlm.nih.gov/17717384
  32. [32]Newville, M. Fundamentals of xafs. Reviews in Mineralogy and Geochemistry 78, 33–74 (2014).DOI
  33. [33]Rehr, J. J. & Albers, R. C. Theoretical approaches to x-ray absorption fine structure. Rev. Mod. Phys. 72, 621–654 (2000). URL https://link.aps.org/doi/10.1103/RevModPhys.72.621.DOI
  34. [34]Rost, C. M., Rak, Z., Brenner, D. W. & Maria, J.-P. Journal of the American Ceramic Society 100, 2732–2738 (2017).
  35. [35]Pu, Y. et al. (mg, mn, fe, co, ni) o: A rocksalt high-entropy oxide containing divalent mn and fe. Science Advances 9, eadi8809 (2023).DOI
  36. [36]D’Ippolito, V., Andreozzi, G. B., Bersani, D. & Lottici, P. P. Raman fingerprint of chromate, aluminate and ferrite spinels. Journal of Raman Spectroscopy 46, 1255–1264 (2015).DOI
  37. [37]Takubo, K. et al. Evolution of phonon raman spectra with orbital ordering in spinel MnV₂O₄. Phys. Rev. B 84, 094406 (2011). URL https://link.aps.org/doi/10.1103/PhysRevB.84.094406.
  38. [38]Tsurkan, V., Von Nidda, H.-A. K., Deisenhofer, J., Lunkenheimer, P. & Loidl, A. On the complexity of spinels: Magnetic, electronic, and polar ground states. Physics Reports 926, 1–86 (2021).DOI
  39. [39]Rudolff, T. et al. Spin-phonon coupling in antiferromagnetic chromium spinels. New Journal of Physics 9, 76 (2007).
  40. [40]Tomiyasu, K., Fukunaga, J. & Suzuki, H. Magnetic short-range order and reentrant-spin-glass-like behavior in CoCr₂O₄ and MnCr₂O₄ by means of neutron scattering and magnetization measurements. Physical Review B 70, 214434 (2004).DOI
  41. [41]Bhowmik, R., Ranganathan, R. & Nagarajan, R. Lattice expansion and noncollinear to collinear ferrimagnetic order in a MnCr₂O₄ nanoparticle. Physical Review B 73, 144413 (2006).DOI
  42. [42]Yamasaki, Y. et al. Magnetic reversal of the ferroelectric polarization in a multiferroic spinel oxide. Physical review letters 96, 207204 (2006).pubmed.ncbi.nlm.nih.gov/16803202
  43. [43]Dey, K., Majumdar, S. & Giri, S. Ferroelectricity in spiral short-range-ordered magnetic state of spinel MnCr₂O₄: Significance of topological frustration and magnetoelastic coupling. Physical Review B 90, 184424 (2014).DOI
  44. [44]Suchomel, M. R., Shoemaker, D. P., Ribaud, L., Kemei, M. C. & Seshadri, R. Spin-induced symmetry breaking in orbitally ordered NiCr₂O₄ and CuCr₂O₄. Physical Review B 86, 054406 (2012).
  45. [45]Dutton, S. E., Huang, Q., Tchernyshyov, O., Broholm, C. & Cava, R. J. Sensitivity of the magnetic properties of the ZnCr₂O₄ and MgCr₂O₄ spinels to nonstoichiometry. Physical Review B 83, 064407 (2011).DOI
  46. [46]Van Der Laan, G., Chopdekar, R., Suzuki, Y. & Arenholz, E. Strain-induced changes in the electronic structure of MnCr₂O₄ thin films probed by x-ray magnetic circular dichroism. Physical review letters 105, 067405 (2010).pubmed.ncbi.nlm.nih.gov/20868013
  47. [47]Kim, I. et al. Electric polarization enhancement in multiferroic CoCr₂O₄ crystals with Cr-site mixing. Applied Physics Letters 94 (2009).DOI
  48. [48]Shannon, R. T. & Prewitt, C. Revised values of effective ionic radii. Acta Crystallographica Section B: Structural Crystallography and Crystal Chemistry 26, 1046–1048 (1970).DOI
  49. [49]Krysko, E. et al. Studies on the structure and the magnetic properties of high-entropy spinel oxide (mgmnfeconi) al2o4. APL Materials 11, 101123 (2023).DOI
  50. [50]Stöhr, J. & Siegmann, H. C. Magnetism. Solid-State Sciences. Springer, Berlin, Heidelberg 5, 236 (2006).
  51. [51]Windsor, Y. W. et al. Magnetic properties of strained multiferroic coc r 2 o 4: A soft x-ray study. Physical Review B 95, 224413 (2017).
  52. [52]Acharyya, S. S., Ghosh, S., Adak, S., Sasaki, T. & Bal, R. Facile synthesis of cucr2o4 spinel nanoparticles: a recyclable heterogeneous catalyst for the one pot hydroxylation of benzene. Catal. Sci. Technol. 4, 4232–4241 (2014). URL http://dx.doi.org/10.1039/C4CY00615A.
  53. [53]Galivarapu, J. K. et al. Effect of size reduction on cation distribution and magnetic transitions in cocr2o4 multiferroic: Exafs, magnetic and diffused neutron scattering measurements. RSC Adv. 6, 63809–63819 (2016). URL http://dx.doi.org/10.1039/C6RA10189F.
  54. [54]Kaplan, T. & Menyuk, N. Spin ordering in three-dimensional crystals with strong competing exchange interactions. Philosophical Magazine 87, 3711–3785 (2007).DOI
  55. [55]Kaplan, T. A. Classical theory of spin configurations in the cubic spinel. Phys. Rev. 119, 1460–1470 (1960). URL https://link.aps.org/doi/10.1103/PhysRev.119.1460.DOI
  56. [56]Winkler, E. et al. Magnetocrystalline interactions in mncr 2 o 4 spinel. Physical Review B 80, 104418 (2009).
  57. [57]Ederer, C. & Komelj, M. Magnetic coupling in Cocr2O4 and Mncr2O4: An LSDA + U study. Phys. Rev. B 76, 064409 (2007). URL https://link.aps.org/doi/10.1103/PhysRevB.76.064409.DOI
  58. [58]Mugiraneza, S. & Hallas, A. M. Tutorial: a beginner’s guide to interpreting magnetic susceptibility data with the curie-weiss law. Communications Physics 5, 95 (2022).DOI
  59. [59]Coey, J. M. D. Magnetism And Magnetic Materials (Cambridge University Press, U.K., 2010).
  60. [60]Kassem, M. A., El-Fadl, A. A., Nashaat, A. M. & Nakamura, H. Structural, optical and single-domain magnetic features of the noncollinear ferrimagnetic nano-spinel chromites acr _2 o _4(a= ni, co, and mn). arXiv preprint arXiv:2305.17856 (2023).arxiv.org/abs/2305.17856
  61. [61]Lee, S.-H., Broholm, C., Kim, T., W Ratcliff, I. & Cheong, S.-W. Local spin resonance and spin-peierls-like phase transition in a geometrically frustrated antiferromagnet. Physical Review Letters 84, 3718 (2000).pubmed.ncbi.nlm.nih.gov/11019185
  62. [62]Ganguly, S., Chimata, R. & Sanyal, B. Overcoming magnetic frustration and promoting half-metallicity in spinel cocr2o4 by doping with fe. Phys. Rev. B 92, 224417 (2015). URL https://link.aps.org/doi/10.1103/PhysRevB.92.224417.DOI
  63. [63]Rák, Z., Maria, J.-P. & Brenner, D. Evidence for jahn-teller compression in the (mg, co, ni, cu, zn) o entropy-stabilized oxide: A dft study. Materials Letters 217, 300–303 (2018).DOI
  64. [64]Rodríguez-Carvajal, J. Recent advances in magnetic structure determination by neutron powder diffraction. Physica B: Condensed Matter 192, 55–69 (1993). URL https://www.sciencedirect.com/science/article/pii/092145269390108I.
  65. [65]Ravel, B. & Newville, M. Athena, artemis, hephaestus: data analysis for x-ray absorption spectroscopy using ifeffit. Journal of synchrotron radiation 12, 537–541 (2005).pubmed.ncbi.nlm.nih.gov/15968136
  66. [66]Kresse, G. & Joubert, D. From ultrasoft pseudopotentials to the projector augmented-wave method. Phys. Rev. B 59, 1758–1775 (1999). URL https://link.aps.org/doi/10.1103/PhysRevB.59.1758.DOI
  67. [67]Kresse, G. & Furthmüller, J. Efficient iterative schemes for ab initio total-energy calculations using a plane-wave basis set. Phys. Rev. B 54, 11169–11186 (1996). URL https://link.aps.org/doi/10.1103/PhysRevB.54.11169.DOI
  68. [68]Perdew, J. P., Burke, K. & Ernzerhof, M. Generalized gradient approximation made simple. Phys. Rev. Lett. 77, 3865–3868 (1996). URL https://link.aps.org/doi/10.1103/PhysRevLett.77.3865.DOI
  69. [69]Dudarev, S. L., Botton, G. A., Savrasov, S. Y., Humphreys, C. J. & Sutton, A. P. Electron-energy-loss spectra and the structural stability of nickel oxide: An lsda+u study. Phys. Rev. B 57, 1505–1509 (1998). URL https://link.aps.org/doi/10.1103/PhysRevB.57.1505.DOI
  70. [70]Das, D. & Ghosh, S. Density functional theory based comparative study of electronic structures and magnetic properties of spinel acr2o4 (a = mn, fe, co, ni) compounds. Journal of Physics D: Applied Physics 48, 425001 (2015). URL https://dx.doi.org/10.1088/0022-3727/48/42/425001.
  71. [71]Wang, L., Maxisch, T. & Ceder, G. Oxidation energies of transition metal oxides within the GGA + U framework. Phys. Rev. B 73, 195107 (2006). URL https://link.aps.org/doi/10.1103/PhysRevB.73.195107.
  72. [72]Himmetoglu, B., Wentzcovitch, R. M. & Cococcioni, M. First-principles study of electronic and structural properties of cuo. Phys. Rev. B 84, 115108 (2011). URL https://link.aps.org/ doi/10.1103/PhysRevB.84.115108.DOI
  73. [73]Harun, K., Salleh, N. A., Deghfel, B., Yaakob, M. K. & Mohamad, A. A. Dft + u calculations for electronic, structural, and optical properties of zno wurtzite structure: A review. Results in Physics 16, 102829 (2020). URL https://www.sciencedirect.com/science/article/pii/S22113797193227287.DOI

Paper details

vlnc:W_zsgbuc6g
Version
v1 · latest
Published
Fresh — added to the Hub within the last 30 days
Added
License
CC BY 4.0
Usage

views · 0

downloads · 0

A view counts once per browser per day, a download each time the PDF is requested.

  • Physics and Astronomy

Not recorded for this paper

View statement
Looking for related papers…
Contents