A Sideways Crack-Path Instability Amplified by Slow Loading
Abstract
Crack-path instabilities in solids are typically associated with high propagation velocities. In contrast, we show that nanoparticle-filled elastomers exhibit a sideways crack-path instability that is amplified as the pulling velocity decreases and nearly vanishes at high pulling velocities. The sideways deviation amplitude decreases logarithmically with increasing pulling velocity and scales as the square root of the filler fraction. Large deviations develop at low mean crack velocities and are associated with effective fracture energies up to two orders of magnitude lower. These findings are consistent with subcritical rupture kinetics and suggest that the deviation amplitude is limited by the elasto-adhesive length.
In homogeneous isotropic solids under Mode-I loading, cracks are generally expected to propagate along a straight path perpendicular to the applied load. At high propagation velocities, this path can become dynamically unstable, leading to oscillatory crack trajectories or microbranching [1, 2, 3]. In heterogeneous brittle materials, disorder can also produce intermittent crack propagation and rough fracture surfaces [4, 5, 6], which may have an impact on fracture energy [7]. Cracks may also be deflected by structural anisotropy toward directions of lower fracture resistance or greater energy release rate [8]. In some tough elastomers, the initially isotropic structure can become anisotropic under large stretch, allowing cracks to propagate sideways, approximately parallel to the loading direction [9, 10]. However, the influence of loading rate on crack-path selection remains unclear, as contrasting rate dependences have been reported for sideways crack propagation in elastomers [10, 11].
In elastomers, crack-path deviations have been observed under various loading conditions. Under tearing conditions, both loading rate and temperature can strongly influence the stability of the crack trajectory [12, 13, 14], while biaxial loading and the resulting molecular orientation may affect sideways crack propagation [15]. Depending on the material and loading conditions, deviations may remain small and produce rough fracture surfaces [16, 17], or develop into large departures from the conventional crack path [10, 18]. Three-dimensional effects may further complicate this behavior in thick elastomer samples [10, 19]. Despite these observations, systematic quantitative measurements of the amplitude and growth dynamics of sideways cracks remain scarce [17].
Here, we systematically quantify sideways crack propagation in nanoparticle-filled elastomers over broad ranges of pulling velocity and filler fraction. We find that, in marked contrast to conventional high-speed crack-path instabilities, this sideways crack-path instability is amplified as the loading rate decreases, while it nearly vanishes at high loading velocities. The deviation amplitude decreases logarithmically with increasing pulling velocity, while the prefactor of this dependence increases approximately as the square root of the filler fraction. Measurements of the growth time show that large deviations develop at much lower mean crack velocities and are associated with effective fracture energies reduced by up to two orders of magnitude. We thus identify a time-dependent crack-path instability whose direction may be selected by stretch-induced structural anisotropy and whose amplitude is controlled by subcritical rupture kinetics. Remarkably, the deviation amplitude always remains below the elasto-adhesive length.
Single edge notch tensile (SENT) specimens with dimensions of length , width and thickness were prepared with a pre-crack of length to control crack initiation (Figure 1). We investigated five PDMS-based elastomer formulations with different silica mass fractions , prepared specifically for this study by Elkem Silicones (Saint-Fons, France) (Table I). The samples were

Figure 1. (a) Schematic drawing of the test used to measure crack deviations . The arrows indicate the loading direction. (b) Typical post-mortem images illustrating these deviations in the notched Si23 sample fractured at pulling velocities from mm.s to mm.s (scale bar: 2 mm).
| Formulation | Si0 | Si5 | Si9 | Si17 | Si23 |
| Rhodorsil Gum 759 (w%) | 100 | 95 | 91 | 83 | 77 |
| Silica Ae55 (w%) | 0 | 5 | 9 | 17 | 23 |
Table 1. Sample formulations, given as the mass fraction of silicone (Rhodorsil® Gum 759) and fumed silica nanoparticles (AE55, Elkem Silicones).
stretched using a custom-built tensile apparatus at constant velocities spanning three orders of magnitude, from to , corresponding to tensile strain rates between and . Once clamped between the machine jaws, each specimen was subjected to a low pre-stress of 0.05 MPa. The applied force was recorded at 100 Hz with an accuracy of . All tests were conducted at room temperature until sample failure. Post-mortem, the sideways crack was imaged using a Canon EOS 100D camera equipped with a Canon EF-S 18 – 55 mm lens, yielding a pixel resolution of . Representative fracture surface images for the Si23 formulation stretched at various pulling velocities show that crack deviations from a straight path are much larger at low velocities (Figure 1).
To quantify crack deviations, we measured the perpendicular distance between the initial notch and the final crack path, as defined in Figure 1. Figure 2(a) shows that, at a fixed pulling velocity, this deviation increases monotonically with filler mass fraction, in contrast to the non-monotonic behavior observed for the tear energy [20, 21]. Conversely, for a given filler content, the crack deviation decreases markedly as the pulling velocity increases over three orders of magnitude. At sufficiently high velocities, deviations become negligible for all filler fractions, although a small residual deviation persists, as observed even in pure PDMS. The observed behavior is approximately described by:

Figure 2. (a) Deviation amplitude as a function of the loading velocity . Lines are linear fits . (b) Evolution of the fitted parameter as a function of the square root of filler mass fraction .
where is a characteristic velocity above which deviations almost vanish. Strikingly, the prefactor increases with the square-root of the filler fraction: (Figure 2(b)).
When comparing the measured fracture energy [21] with the crack deviation amplitude (Figure 3), we observe a general tendency of the tear energy to decrease with increasing deviation. This trend is especially obvious at the highest filler fraction (). These results challenge the common assumption that crack deviation enhances material strength; on the contrary, they suggest that deviations correlate with reduced tear resistance.

Figure 3. Tear energy of pre-notched samples as a function of deviation amplitude . Lines are guides to the eye, drawn with the slope obtained from the fit at . The blue horizontal line indicates the tear-energy level of pure PDMS.
To better understand how crack deviations develop and why they tend to reduce the overall tear energy, we first estimate their mean growth velocity as , where is the time to rupture. We find that the deviation velocity is one to two orders of magnitude lower than the imposed pulling velocity (Figure 4). As shown in the inset of Figure 4, the ratio is larger at lower pulling velocities, indicating that crack deviations grow more readily under slow loading. This suggests that time-dependent rupture processes occurring under subcritical conditions, below the nominal failure threshold, contribute to the growth

Figure 4. Sideway crack velocity as a function of the imposed displacement velocity ranging from to . Inset: Normalized sideways crack velocity.
of the deviations. Such processes are typically thermally activated and may enable fracture at lower tear energies.
To estimate the fracture energy specifically associated with sideways crack growth, we determine the mechanical energy released during this process [21]. We find that decreases with increasing deviation amplitude, with long deviations exhibiting values one to two orders of magnitude lower than short deviations (Figure 5). This result is consistent with large deviations developing through time-dependent rupture mechanisms that become accessible when sufficient time is available. For long deviations, the fracture energy approaches that of the unfilled silicone [21], thereby effectively suppressing the reinforcing effect of the filler. Although strongly depends on the deviation amplitude, it exhibits no clear dependence on filler content. Its variation is approximately described by

Figure 5. Fracture energy associated to sideways crack growth as a function of the crack deviation amplitude .
with and .
Combining Eq. (1) and (2) leads to a power-law dependence on pulling velocity:
where . Such small exponents are typical of polymer fracture dynamics and are commonly attributed to rate-dependent rupture processes [12, 18, 22, 23, 24, 25]. The exponent has been reported to increase with filler content [26], consistently with the increase in the parameter with filler fraction observed here. Thus, the power-law dependence of the fracture energy on the pulling velocity further supports the interpretation of crack deviations as a manifestation of a rate-dependent growth process. Furthermore, recent simulations of hyperelastic materials show that the elastic energy release rate for sideways cracks decreases with increasing crack length [10]. A decrease in with deviation amplitude, as observed experimentally (Figure 5), is therefore necessary to allow the propagation of large sideways cracks despite the decreasing energy release rate.
A central quantity governing fracture in soft polymers is the elasto-adhesive length, defined as , where is the elastic modulus of the elastomer [27]. This length compares the energy required to create new surfaces with the elastic energy density and sets the spatial
extent of the region surrounding the crack tip in which elastic strains become of order unity. Consequently, even in simple elastomers such as unfilled PDMS, linear elasticity necessarily breaks down at distances comparable to .
For each filled formulation, the crack-path deviation amplitude is systematically smaller than the elasto-adhesive length calculated using the fracture energy of the corresponding filled elastomer (Figure 6 and [21]). However, the two quantities are not directly correlated. While depends only weakly on the pulling velocity, decreases markedly with increasing pulling velocity. Their dependences on filler content also differ. At the highest filler mass fraction, , decreases, whereas continues to increase. Thus, does not determine the deviation amplitude, although the systematic inequality suggests that it may provide an upper bound.

Figure 6. Crack deviation amplitude normalized by the elasto-adhesive length as a function of .
A distinct set of observations concerns pure PDMS. Small crack deviations of approximately are observed even without fillers (Figure 2), consistent with their amplitude being bounded by the elasto-adhesive length of pure PDMS, (Figure 6). Furthermore, the characteristic length introduced by Eq. (2) is approximately independent of filler content and is comparable to . The effective fracture energy associated with large sideways cracks also approaches that of pure PDMS [21]. These observations suggest that, over sufficiently long timescales, sideways crack growth in the filled elastomers becomes increasingly influenced by the fracture response of the pure PDMS matrix. The physical origin of the similarities between these characteristic length scales nevertheless remains unclear.
Although subcritical rupture kinetics appear to control the amplitude of the sideways crack instability, they do not explain why cracks propagate along the loading direction rather than perpendicular to it. Several mechanisms may account for this directional selection. First, recent studies have shown that solid inclusions modify the local strain-energy density, favoring propagation along directions of maximum energy density, which may differ from the expected Mode I direction [28]. Second, experiments on strain-crystallizing elastomers have shown that polymer dynamics accelerate in regions ahead of sideways cracks, promoting growth along specific directions aligned with the loading direction [29].
At a fixed pulling velocity, the rupture time does not vary much with filler fraction because the macroscopic stretch at break is similar for the different formulations. Thus, the increase in deviation amplitude with filler fraction cannot be attributed primarily to a longer time available for sideways crack growth. However, higher filler fraction will concentrate more deformation in the polymer matrix, causing some regions between filler aggregates to reach larger local stretches. This could allow subcritical sideways cracks to propagate farther within approximately the same rupture time. This interpretation remains qualitative and does not explain the observed square-root dependence on filler fraction.
In conclusion, our results show that sideways crack deviations in nanoparticle-filled elastomers are strongly influenced by both filler content and pulling velocity. Increasing the filler fraction produces larger deviation amplitudes, whereas increasing the pulling velocity suppresses the instability, with deviations nearly vanishing at high velocities. Contrary to the common expectation that crack deflection enhances toughness, the macroscopic tear energy decreases as the deviation amplitude increases. The fracture energy associated with sideways propagation also decreases with the mean crack velocity and approaches that of pure PDMS for the slowest-growing cracks. This result may have important implications for the long-term durability of filled elastomers since their resistance to slow rupture may ultimately be governed by the fracture properties of the polymer matrix rather than those of the reinforced material.
Acknowledgments
The authors acknowledge the support of the French National Research Agency (ANR) under grant ANR-12-BS09-014 (StickSlip), and thank Elkem Silicones for providing filled elastomer samples. All data supporting the findings of this study are openly available here [30].
Corresponding author: [email protected]
References
Supplemental Material
For the various material formulations and test conditions, this Supplemental Material reports the stress and stretch ratio at failure measured on unnotched samples, the procedure used to estimate the fracture energy associated with sideways crack growth, and the calculated elasto-adhesive lengths.
Fracture energy dependence on filler fraction and loading velocity
Stress versus stretch ratio data at the breaking point, , are shown in Figure 7a for pre-notched specimens. These data correspond to unfilled samples () and filled samples with silica mass fractions , tested at room temperature over strain rates ranging from to . The addition of silica generally enhances the mechanical strength, although this effect becomes non-monotonic at high filler contents. In particular, at the highest filler content (), the strength decreases to values comparable to those of moderately filled samples (). This non-monotonic trend has also been reported in previous studies of filled elastomers [20].

Figure 7. (a) Stress-elongation ratio curves at the breaking point, , for pre-notched samples () at different strain rates. (b) Tear energy, , of the pre-notched samples, for different formulations and loading velocities ranging from to .
To estimate the fracture energy , we consider the energy release rate during crack advance, which is defined as the variation in mechanical energy per unit increase in fracture surface area. For a SENT specimen, is given by [18]:
where is the initial notch length, the stretch ratio in the uniformly deformed region and the elastic energy density in the same region (i.e. far from the crack tip), both evaluated at the breaking point. The values of as a function of tensile velocity for each formulation are shown in Figure 7b. Unfilled samples have a typical tear energy of , while filled samples exhibit tear energies 10 to 40 times larger.
Fracture energy of crack deviations
To estimate the fracture energy specifically associated to sideways cracks, we determine the amount of mechanical energy released during the growth of the sideways crack. To that end, we compare the stored elastic energy in two sample configurations at a fixed stretch ratio . In the first configuration, a notched sample strained to stores an elastic energy . This quantity cannot be directly measured if a crack has already initiated and begun to deviate at deformation . To estimate , we use stress-strain data from tensile tests on unnotched samples and rescale the curves to match the initial elastic response of the notched sample, prior any crack growth (Figure 8). In the second configuration, a notched sample at the same deformation, but with a developed crack deviation, stores a smaller elastic energy, . The difference in elastic energy represents the elastic energy dissipated due the growth of a crack deviation. At the rupture stretch ratio , and assuming the deviation extends over a distance , we estimate the fracture energy associated with crack deviation as:

Figure 8. Curve rescaling to match the initial elastic response of the notched sample to evaluate the fracture energy associated with crack deviation, example for and (see text for details).
where is the sample thickness.
Estimate of the elasto-adhesive length

Figure 9. (a) Elastic modulus as a function of loading rate for various filler fractions. (b) Elasto-adhesive lengths determined from the loading rate and filler dependent elastic modulus and fracture energy.
The elasto-adhesive length is defined as , where is the filler-dependent fracture energy shown in Figure 7(b) and is the small-strain Young’s modulus. To determine , we fit the low-strain portion of the stress-strain curves measured on unnotched samples using the hyperelastic Mooney-Rivlin model , and set . Because the stress-strain curves depend on the pulling velocity, the elastic modulus increases slightly and approximately logarithmically with pulling velocity, as commonly observed in polymers. For the filled formulations, the elasto-adhesive length is typically of the order of 10 mm or larger, whereas it is approximately mm for unfilled PDMS. In all cases, for a given filler fraction and pulling velocity, it exceeds the corresponding crack-deviation amplitude.
References
- [1]E. Bouchbinder, T. Goldman, and J. Fineberg, Reports on Progress in Physics 77, 046501 (2014).
- [2]C.-H. Chen, E. Bouchbinder, and A. Karma, Nature Physics 13, 1186 (2017).
- [3]I. Kolvin, J. Fineberg, and M. Adda-Bedia, Physical Review Letters 119, 215505 (2017).
- [4]S. Santucci, L. Vanel, and S. Ciliberto, Physical Review Letters 93, 095505 (2004).
- [5]N. Mallick, P. P. Cortet, S. Santucci, S. G. Roux, and L. Vanel, Physical Review Letters 98, 255502 (2007).
- [6]D. Bonamy and E. Bouchaud, Physics Reports 498, 1 (2011).
- [7]J. Scheibert, C. Guerra, F. Célarié, D. Dalmas, and D. Bonamy, Physical Review Letters 104, 045501 (2010).
- [8]V. Hakim and A. Karma, Phys. Rev. Lett. 95, 235501 (2005).
- [9]A. N. Gent, M. Razzaghi-Kashani, and G. R. Hamed, Rubber Chem. Technol. 76, 122 (2003).
- [10]S. Lee and M. Pharr, Proc. Natl. Acad. Sci. 116, 9251 (2019).
- [11]S. Gherib, L. Chazeau, J. M. Pelletier, and H. Satha, J. Appl. Polym. Sci. 118, 435 (2010).
- [12]H. W. Greensmith, J. Polym. Sci. 21, 175 (1956).
- [13]R. G. Stacer, L. C. Yanyo, and F. N. Kelley, Rubber Chem. Technol. 58, 421 (1985).
- [14]R. G. Stacer and F. N. Kelley, Rubber Chem. Technol. 58, 924 (1985).
- [15]C. Marano, R. Calabrò, and M. Rink, J. Polym. Sci., Part B: Polym. Phys. 48, 1509 (2010).
- [16]K. Tsunoda, J. J. C. Busfield, C. K. L. Davies, and A. G. Thomas, J. Mater. Sci. 35, 5187 (2000).
- [17]B. Gabrielle, L. Guy, P. A. Albouy, L. Vanel, D. R. Long, and P. Sotta, Macromolecules 44, 7006 (2011).
- [18]G. Lake, A. Samsuri, S. Teo, and J. Vaja, Polymer 32, 2963 (1991).
- [19]N. Xue, R. Long, E. R. Dufresne, and R. W. Style, Phys. Rev. X 14, 011054 (2024).
- [20]J. G. de Castro, R. Zargar, M. Habibi, S. H. Varol, S. H. Parekh, B. Hosseinkhani, M. Adda-Bedia, and D. Bonn, Appl. Phys. Lett. 106, 221904 (2015).
- [21]See Supplemental Material at [URL] for details of the experimental characterizations.
- [22]D. Maugis and M. Barquins, J. Phys. D-Appl. Phys. 11, 1989 (1978).
- [23]R. Stacer, E. von Meerwall, and F. Kelley, Rubber Chem. Technol. 58, 913 (1985).
- [24]A. N. Gent, Langmuir 12, 4492 (1996).
- [25]M. Barquins and M. Ciccotti, Int. J. Adhes. Adhes. 17, 65 (1997).
- [26]Y. Morishita, K. Tsunoda, and K. Urayama, Phys. Rev. E 93, 043001 (2016).
- [27]C. Creton and M. Ciccotti, Rep. Prog. Phys. 79, 046601 (2016).
- [28]L. Rozen-Levy, J. M. Kolinski, G. Cohen, and J. Fineberg, Phys. Rev. Lett. 125, 175501 (2020).
- [29]J. Ju, G. E. Sanoja, M. Y. Nagazi, L. Cippelletti, Z. Liu, C. Y. Hui, M. Ciccotti, T. Narita, and C. Creton, Phys. Rev. X 13, 021030 (2023).
- [30]G. Pallares, O. Ramos, and L. Vanel, 10.5281/zenodo.23361968 (2026).