betaFeedback

WorksPhysics and Astronomy

Heterogeneous superconductivity emerging from a charge-stripe state in kagome lattices

Abstract

Charge density wave (CDW) and superconductivity have long been recognized as competing orders. However, recent achievements establish that the interplay between these two collective electronic phenomena can be more perplexing, with emergent phenomena arising from their cooperation. Here we report a distinctive case of the kagome superconductors CsV3Sb5-xSnx, in which the characteristics of superconductivity evolve in accordance with the form of CDW order. As the triple-Q CDW in CsV3Sb5 transforms to a short-range stripelike CDW at xc = 0.07, a sudden change in superconducting properties occurs concomitantly. A combination of thermodynamic, electrical transport and scanning tunneling microscopy experiments reveals a heterogeneous superconducting state beyond xc: the superconducting gap exhibits pronounced spatial variation, in conformity with a distribution of critical temperature and the resulted superconducting precursor effects. Moreover, abundant normal fluid persists deep into the superconducting state, as evidenced by remnants of electronic specific heat and zero-energy quasiparticle interference. These observations are unrelated to the chemical inhomogeneity and residual strain effect introduced by Sn substitution. Instead, they emulate the phenomenology that a sign-changing superconducting order parameter is subject to strong pair-breaking scattering with the short-range charge stripes and hence reflect the unconventional nature of superconductivity developing inside the charge-stripe state.

Introduction

The phase diagrams of quantum materials are often delineated by the presence of multiple electronic orders. Charge density wave (CDW) and superconductivity, two typical symmetry-breaking electronic instabilities, compete with each other according to conventional wisdom. Recent studies, however, have revealed more complicated relationships between these orders in many categories of superconductors [1, 2, 3, 4, 5, 6]. In high-temperature cuprate superconductors, short-range CDW ubiquitously coexists with superconductivity [2, 3, 4], and dynamic CDW correlations may be involved in dd-wave pairing [7]; in certain members such as underdoped YBa2Cu3O6+δ\mathrm{YBa_2Cu_3O_{6+\delta}} (YBCO), long-range CDW order can be induced by intense magnetic fields (HH) [8, 9] and an anomalous vortex liquid phase with “resilient” superconducting behavior arises from its coupling with superconductivity [10, 11]. Moreover, the intertwinement between CDW and superconductivity promotes exotic pairing states such as pair density wave (PDW) in both high-temperature [1, 12, 13] and conventional [5, 14] superconductors. The recently discovered kagome-lattice superconductor CsV3Sb5\mathrm{CsV}_{3}\mathrm{Sb}_{5} [15] serves as an ideal candidate for exploring the complex interplay between electronic orders. It exhibits a triple-QQ CDW state with an onset temperature TCDW=94T_{\mathrm{CDW}} = 94 K [15]; the CDW adopts an in-plane 2×22 \times2 superlattice and mixing 2×2×22 \times2 \times2 and 2×2×42 \times2 \times4 stacking along cc axis [16, 17, 18]. Superconductivity develops inside the CDW state with a transition temperature Tc≈3.0T_c \approx3.0 K, characterized by an anisotropic full superconducting gap (Δ\Delta) [19, 20, 21].

The coexisting superconductivity and CDW in CsV3Sb5\mathrm{CsV}_{3}\mathrm{Sb}_{5} can be effectively manipulated via applying pressure (pp) or chemical doping. The TT-pp phase diagram is marked by two critical pressures of Pc1≈0.7P_{c1} \approx0.7 GPa and Pc2≈2.0P_{c2} \approx2.0 GPa [22, 23]; at Pc1P_{c1}, the triple-QQ CDW is replaced by a unidirectional (single-QQ) form thus called a stripelike order, which is fully suppressed at Pc2P_{c2} [23, 24]. TcT_c is enhanced at each transition, rendering a double-peak superconducting dome in the TT-pp phase diagram [22, 23]. Substituting the V atoms in the kagome plane with Ti, Nb or Ta can monotonically suppress the triple-QQ CDW and boost TcT_c, eventually leading to an isotropic superconducting gap in the undistorted kagome phase [25, 26, 27]. By contrast, hole doping via substitution of Sn onto the in-plane Sb sites produces a phase diagram mimicking the TT-pp phase diagram, underscored by the double-dome superconductivity and the presence of single-QQ stripelike CDW beyond the minima of TcT_c [28, 29, 30] (Figure 1a-Figure 1c). Intriguingly, the pressure-induced and Sn-doping-induced charge stripe orders have similar periodicities; the former is a long-range order [24], whereas the latter is short-ranged (with an anisotropic correlation length ξCDW∼6\xi_{\mathrm{CDW}} \sim6-1818 nm at x=0.15x = 0.15 [29]) and gradually becomes fluctuating upon increase of xx [30, 31]. The nonmonotonic pressure/Sn-doping dependence of superconductivity and its correspondence to the transformations of CDW highlight the intimate link between the two orders, strongly implying that their involved mutual relation is not simply competitive.

Phase diagram of CsV₃Sb₅₋ₓSnₓ and characteristic temperatures of superconductivity

Figure 1. Phase diagram of CsV₃Sb₅₋ₓSnₓ and the characteristic temperatures of superconductivity. a, Charge-density-wave (CDW) patterns in the kagome vanadium network: (left) triple-QQ 2×22 \times2 CDW and (right) the stripelike single-QQ CDW [30]. Arrows denote the CDW wavevectors. b, c, electronic phase diagram of CsV₃Sb₅₋ₓSnₓ showing the evolution of the CDW (b) and superconductivity (c) upon increase of Sn doping level xx. Different colours in b discriminate the CDW phase regions with stars representing the transition temperature TCDWT_{\mathrm{CDW}} determined from resistivity (Supplementary Fig. 3). Note that the single-QQ CDW in b is a short-range order; the corresponding phase regime (II, orange-shaded) crossover to a nearly-undistorted kagome phase (III) with fluctuating single-QQ charge correlation, as denoted by the colour gradient. Circles, hexagons and squares in c represent the onset temperatures of diamagnetism (TdT_{\mathrm{d}}), specific heat anomaly (TcST_{\mathrm{c}}^{\mathrm{S}}) and zero resistivity (Tc0T_{\mathrm{c0}}), respectively. d-o, In-plane resistivity ρxx\rho_{xx} (d, g, j, m), volume magnetic susceptibility χv\chi_{\mathrm{v}} (e, h, k, n) and electronic specific heat Ce/TC_{\mathrm{e}}/T (f, i, l, o, see Methods for the extraction of CeC_{\mathrm{e}}) plotted as a function of temperature (TT) for samples with x=0.06x = 0.06 (d-f, T≤4T \le4 K), 0.07 (g-i, T≤4T \le4 K), 0.09 (j-l, T≤4T \le4 K) and 0.12 (m-o, T≤4T \le4 K). χv\chi_{\mathrm{v}} was measured with a magnetic field of 5 Oe applied along the cc axis and was corrected for the demagnetizing effects; both zero-field-cooled (ZFC, olive) and field-cooled (FC, blue) data are shown. Vertical dashed lines indicate the characteristic temperatures Tc0T_{\mathrm{c0}}, TcST_{\mathrm{c}}^{\mathrm{S}} and TdT_{\mathrm{d}} for each sample.

In this work, we utilize complementary probes of electrical transport, torque magnetometry, specific heat and scanning tunneling microscopy (STM) to explore the evolution of superconductivity upon Sn doping in CsV3Sb5−xSnx\mathrm{CsV}_{3}\mathrm{Sb}_{5-x}\mathrm{Sn}_{x} up to x≈0.30x \approx0.30 (where the charge stripes are likely of the fluctuating type). A peculiar heterogeneous superconducting state possessing (i) a distribution of local TcT_c, (ii) a spatially inhomogeneous Δ\Delta and (iii) a large population of unpaired electrons is identified, emerging uniquely from the (short-range) single-QQ CDW phase. These unusual signatures are irrelevant to the chemical disorder and residual strain effect from Sn doping, but are most likely to stem from the strong influence of pair-breaking scattering with the presence of short-range charge stripe [32]; such intense nonmagnetic pair breaking is in stark contrast to the expectation for conventional Bardeen-Cooper-Schrieffer (BCS) superconductors [33], instead being a hallmark of sign-reversal superconductivity. A phenomenological resemblance between this state and the overdoped high-TcT_c cuprates [34, 35, 36, 37] underpins the realization of unconventional superconductivity in CsV3Sb5−xSnx\mathrm{CsV}_{3}\mathrm{Sb}_{5-x}\mathrm{Sn}_{x} in the intermediate doping range where the static stripelike CDW prevails.

Results

The electronic phase diagram of CsV3Sb5−xSnx\mathrm{CsV}_{3}\mathrm{Sb}_{5-x}\mathrm{Sn}_{x}

Single crystals of CsV3Sb5−xSnx\mathrm{CsV}_{3}\mathrm{Sb}_{5-x}\mathrm{Sn}_{x} (x=0x = 0, 0.060.06, 0.070.07, 0.090.09, 0.120.12 and 0.300.30) were grown via flux method (Methods and Supplementary Note 1). A TT-xx phase diagram (Figure 1b and Figure 1c) is constructed based on a combination of electrical resistivity (ρ\rho), magnetic susceptibility (χ\chi) and specific heat (CC) measurements. With the inference from previous results [29, 30, 31], three phase regions can be identified: (I) a long-range triple-QQ CDW phase up to x=0.06x = 0.06 (the turquoise shaded region in Figure 1b), characterized by the in-plane 2×22 \times2 superlattice (Figure 1a, left), (II) a single-QQ CDW phase featured by short-range [29], static stripelike CDW with periodicity λ∼3a0\lambda\sim3a_0 [30] (a0a_0 is the in-plane lattice parameter, see Figure 1a, right), commencing at x=0.07x = 0.07 (the orange shaded region in Figure 1b), which crossovers to (III) a phase regime harboring very short-ranged single-QQ charge correlation, developed at x≥0.12x \ge0.12, as illustrated by a fade-out of the orange shades in Figure 1b. The CDW-transformation transition between phases I and II, occurring at xc=0.07x_{\mathrm{c}} = 0.07, is concomitant with a sudden drop in TcT_{\mathrm{c}}: the zero-resistivity onset (Tc0T_{\mathrm{c0}}) decreases from 3.3 K for x=0.06x = 0.06 to 1.2 K for x=0.07x = 0.07 (Figure 1d and Figure 1g), underlining the strong influence of charge order on superconducting pairing. The CDW transition in phase II is ostensibly absent in thermodynamics [28, 29], in accordance with the weak structural impact of the short-range stripelike order; nonetheless, TCDWT_{\mathrm{CDW}} can be determined from an anomaly in dρ/dTd\rho/dT (Supplementary Fig. 3b) and the unidirectional band folding due to the stripelike CDW is clearly manifested in the quasiparticle interference (QPI) in this phase [30]. With further increase of xx, the correlation length of stripelike CDW becomes even shorter, resulting in fluctuating-type charge order [31] in phase III, wherein both the CDW transition in dρ/dTd\rho/dT and the QPI features of the stripe-induced electronic band reconstruction are unresolvable (Supplementary Note 2). As such, we infer that the electronic structure in phase III is almost identical to the undistorted kagome lattice. The overall evolution of superconductivity upon Sn doping is nonmonotonic, with pronounced suppression of Tc0T_{\mathrm{c0}} occurring only in the narrow phase region II (x=0.07x = 0.07-0.090.09) where static short-ranged charge stripe order that suffices to cause band reconstruction (Figure 1b and Figure 1c); a higher Tc0=2.8T_{\mathrm{c0}} = 2.8 K is recovered at the onset of phase III at x=0.12x = 0.12.

Anomalous superconducting state in stripe-ordered CsV₃Sb₅₋ₓSnₓ

A comparison of ρ(T)\rho(T), χ(T)\chi(T) and C(T)C(T), summarized in Figure 1d-Figure 1o (see Supplementary Fig. 3 for data of undoped CsV₃Sb₅ and the x=0.30x = 0.30 sample), further divides the six samples into two groups with distinct superconducting state properties. The first group includes members in phase regimes I (x=0x = 0, $0.06$) and III (x=0.12x = 0.12, 0.300.30). Their superconducting states behave ordinarily: Tc0T_{\mathrm{c0}} coincides with the onsets of both the Meissner diamagnetism (TdT_{\mathrm{d}}) and the specific heat anomaly (TcsT_{\mathrm{c}}^{\mathrm{s}}), signaling the occurrence of a single transition at this critical temperature (Figure 1d-Figure 1f, Figure 1m-Figure 1o, Supplementary Fig. 3c-h). On the contrary, superconducting states in the stripe-ordered compounds in phase II (x=0.07x = 0.07, 0.090.09) show remarkably differentiated characteristic temperatures for the three physical quantities (Figure 1c). Concretely, for x=0.07x = 0.07 (0.090.09), diamagnetism appears at a relatively high Td≈2.4T_{\mathrm{d}} \approx2.4 K (3.53.5 K) and develops a drastic enhancement at Tcs=1.7T_{\mathrm{c}}^{\mathrm{s}} = 1.7 K (2.12.1 K) where the transition in C(T)C(T) occurs, yet ρ\rho becomes zero only at Tc0=1.2T_{\mathrm{c0}} = 1.2 K (2.02.0 K), as displayed in Figure 1g-Figure 1i (Figure 1j-Figure 1l). In addition, the resistive transitions in these two compounds are considerably broadened compared with the first group (Supplementary Fig. 3a); a nonohmic voltage-current (VV-II) relation, manifested as a current-dependent ρ(T)\rho(T) profile, is observed at the transition and extends to ≃1\simeq1 K above $T_{\mathrm{c0}} ({xref}Fig. 1g and j`).

The unusual superconducting behavior uniquely develops in phase region II cannot be assigned to the phase separation prompted by chemical inhomogeneity (e.g., clustering of Sn dopants) or residual strain fields, considering its immediate disappearance at x=0.06x = 0.06 and x=0.12x = 0.12. This inference is further confirmed by the STM results discussed below. Filamentary superconductivity [38] is also irrelevant: The formation of superconducting filaments typically renders Tc0T_{\mathrm{c0}} higher than the onsets of thermodynamic transitions (TdT_{\mathrm{d}} and TcsT_{\mathrm{c}}^{\mathrm{s}}). Intriguingly, there are a few phenomenological parallels between these nonmagnetic, weakly-correlated superconductors and the high-TcT_{\mathrm{c}} cuprates that employ similar signatures: (1) The large disparity between Tc0T_{\mathrm{c0}} and TdT_{\mathrm{d}} (Figure 1c), indicative of appreciable precursor superconducting diamagnetism (χd\chi_{\mathrm{d}}) [35, 39, 40]; (2) the rounded onset of resistive transition resulted from the excess conductivity (paraconductivity) Δσ\Delta\sigma introduced by superconducting precursor [41, 42, 43] and (3) the nonohmic resistivity drop, which is reminiscent of the “fragile” superconductivity [10, 44] emerging due to an intricate compromise between superconductivity and CDW order [11].

Percolative superconducting precursor

Two possible origins of the superconducting precursors, i.e., fluctuating Cooper pairs [39, 41, 45] and percolation process [39, 40, 42, 43], have been scrutinized in previous studies (mostly in high-TcT_c superconductors). The former signifies fluctuations of the superconducting order parameter, happening in both its amplitude (Gaussian fluctuation) and phase [41, 45, 46]; the latter considers a spatial distribution of the superconducting order parameter and, consequently, TcT_c [32, 35, 42]. In the percolation scenario, the development of superconductivity upon cooling is an incremental process, i.e., the growth and eventual proliferation of superconducting clusters embedded in the normal metal medium [42, 43].

The two contributions can be distinguished by their TT evolutions. Gaussian-type fluctuations engender an approximately power-law TT dependence of Δσ\Delta\sigma and χd\chi_d (the Aslamazov-Larkin expressions, Supplementary Note 4) within the framework of Ginzburg-Landau (GL) theory [45], whereas the phase fluctuations are amenable to analysis in the Halperin-Nelson formalism which considers vortex-like excitations [41, 46] (Supplementary Note 4). By contrast, the percolation process, commonly described using the effective-medium theory (EMT), is characterized by the exponential decay of Δσ\Delta\sigma and χd\chi_d with increasing TT [39, 40, 42, 43]. We employed these approaches for superconducting fluctuations and the percolation scenario to our data for CsV3_3Sb5−x_{5-x}Snx_x (x=0.07x = 0.07 and 0.090.09), as denoted by the fitting curves and simulations presented in Fig. 2a-d; the superconducting precursor herein unambiguously stems from the percolation process between T≃(1.0T \simeq(1.0-1.2)Tcs1.2)T_c^s and ≃3.5\simeq3.5 K. In this temperature range, both Δσ\Delta\sigma and χd\chi_d decrease in a roughly exponential fashion with increasing TT, a trend satisfyingly captured by the EMT approach (Methods, more detail in Supplementary Note 5) assuming a significant distribution width of TcT_c (Ξ1≃1.2\Xi_1 \simeq1.2 K and 0.60.6-0.70.7 K for x=0.07x = 0.07 and 0.090.09, respectively, Supplementary Note 5 and Supplementary Figure 5 and Supplementary Figure 5). Conversely, neither the Aslamazov-Larkin model (orange curves) nor the Halperin-Nelson model (wine curves) succeeds in reproducing the amplitude and TT dependence of the precursor superconducting effects (Fig. 2a-d). Hence, we conclude that the fluctuation effect is negligible in CsV3_3Sb5−x_{5-x}Snx_x compared with the influence of the local TcT_c distribution.

EMT analysis of the paraconductivity in CsV$_3$Sb$_{5-x}$Sn$_x$

Supplementary Figure 5. The EMT analysis of the paraconductivity in CsV3_3Sb5−x_{5-x}Snx_x (x=0.07x = 0.07 and 0.090.09). a, The two-component distribution g(T)g(T) of local superconducting transition temperature TcT_{\mathrm{c}}: g(T)=ug1(T)+(1−u)g2(T)g(T) = u g_1(T) + (1-u)g_2(T), with uu being a weighing factor; g1(T)g_1(T) (olive) and g2(T)g_2(T) (blue) are two Gaussians with the same mathematical expectation T0T_0 and half-width-at-half-maximum (HWHM) Ξ1\Xi_1 and Ξ2\Xi_2, respectively (Ξ1>Ξ2\Xi_1 > \Xi_2 as illustrated by the vertical dashed lines). See Methods for more detail. b, The volume fraction of superconducting clusters PP at a temperature TT given by integrating g(T′)g(T^\prime) from T′=TT^\prime= T to +∞+\infty. Here we adopted the fitting parameters that are applied to the x=0.09x = 0.09 sample (main text Fig. 2c): T0=2.0T_0 = 2.0 K, Ξ1=0.65\Xi_1 = 0.65 K, Ξ2=0.2\Xi_2 = 0.2 K and u=0.01u = 0.01. Red vertical dashed lines in a and b indicate the temperature at which the distribution g2g_2 (presumably stems from the proximity effect and inter-grain Josephson coupling) becomes unimportant. c, d, Contrasting the simulations of EMT model utilizing varying parameters Ξ1\Xi_1 and Ξ2\Xi_2 with the data of paraconductivity for x=0.07x = 0.07 (c) and x=0.09x = 0.09 (d). Here uu is fixed at 0.001 in c and 0.01 in d, referring to the superconducting volume fraction estimated from diamagnetic susceptibility (main text Fig. 1). e, f, A contrast of the transverse magnetization M⊥(H)M_{\perp}(H) (e) derived from torque magnetometry (Methods) and ρxx(H)\rho_{xx}(H) (f) measured in a CsV3_3Sb4.93_{4.93}Sn0.07_{0.07} sample at T=0.4T = 0.4 K. HH is applied within the abab plane. Inset of e displays the full hysteresis loops of M⊥M_{\perp}. Vertical dashed line marks the onset field of zero resistivity.

The presence of self-organized puddles wherein the superconductivity is more persistent than their surroundings is further confirmed by contrasting the profiles of magnetoresistance (MR) and magnetization M(H)M(H). In most superconductors, the hysteresis loop of diamagnetism arising from shielding currents only occurs within the vortex solid phase, in which the resistivity is essentially zero at small excitations [47]; the irreversibility field HirrH_{\mathrm{irr}} thus approximately coincides with the onset of nonzero ρ(H)\rho(H). For CsV3_3Sb5−x_{5-x}Snx_x with x=0.09x = 0.09 (Fig. 2e and f) and 0.070.07 (Supplementary Figure 5 and Supplementary Figure 5), however, the magnetization hysteresis closes at a position where MR almost reaches its normal-state values. The concurrence of irreversible diamagnetism and heavily dissipative transport strongly implies a picture of heterogeneity that disconnected superconducting grains scatter inside a metallic environment. As such, the nonohmic resistivity drop (Figure 1g and Figure 1j) reflects current-induced breaking of superconducting inter-grain links [48].

Our two-component EMT modeling (Methods), though being oversimplified, provide a good depiction of the paraconductivity as shown in Fig. 2a and c (note that the EMT analysis does not account for the characteristic size of the superconducting grains, Supplementary Note 5). Based on this, we propose a phenomenological understanding (Fig. 2g-i) of how superconductivity emerges in the stripe-ordered CsV3_3Sb5−x_{5-x}Snx_x: Small-sized superconducting grains appear at T≳TdT \gtrsim T_d (Fig. 2g) and grow in a percolative manner with decreasing TT; at T≃TcsT \simeq T_c^s, proximity effect (depicted by a second component of distribution with scale Ξ2\Xi_2 in the EMT analysis, see Methods and Supplementary Figure 5) drives a large portion of the surrounding medium superconducting (Fig. 2h), giving rise to the drastic enhancement of χd\chi_d and onset of bulk transition in C(T)C(T); a superconducting path across the sample (Fig. 2i) is eventually established at Tc0T_{\mathrm{c0}}. It should be noticed that before the Ξ2\Xi_2 term kicks in, the Ξ1\Xi_1 distribution only contributes to about 0.1% of the total volume fraction (Supplementary Figure 5), hence the high-TcT_{\mathrm{c}} “tail” may evade the detection of many experimental probes.

Visualization of inhomogeneous superconductivity

Spectroscopic-imaging STM probes the spatial characteristics of electronic orders, with which the proposed heterogeneous superconductivity as well as its potential origin can be revealed. To this end, we performed dilution-refrigerator-based STM studies for x=0.09x = 0.09 with a lattice temperature of 20 mK. Figure 3a shows the topography of a 70 nm ×\times 10 nm antimony surface, where the atomic position of individual Sn dopant, substituted for the in-plane Sb atom, is clearly identified (Fig. 3b). The statistically homogeneous distribution of Sn dopants is remarkable: we did not find any propensity for them to form clusters; their concentration was appreciably uniform across seven measured samples (Supplementary Note 1). The normal-state electronic density of states (DOS), reflected by integrating the differential conductance (dI/dV\mathrm{d}I/\mathrm{d}V) between energy windows of ±6\pm6 (Fig. 3c) and ±50\pm50 meV (Fig. 3d), shows no significant spatial inhomogeneity (also see Supplementary Fig. 2). However, the superconducting characteristics, provided by the gap amplitude Δ(r)\Delta(r) and the gap depth H(r)H(r) (defined Fig. 3j, see also Methods and Supplementary Note 6), exhibit pronounced real-space variations (Fig. 3e and f). The gradual variation observed for both Δ(r)\Delta(r) and H(r)H(r) marks a clear departure from the homogenous spatial distributions of Sn atoms and the normal state DOS (Fig. 3c, d and k). Statistical analysis of Δ(r)\Delta(r) yields a mean gap value of Δˉ=323\bar{\Delta} = 323 µeV with a standard deviation of σ=16.6\sigma= 16.6 μeV (Fig. 3g). The resulting σ/Δˉ≈0.051\sigma/\bar{\Delta} \approx0.051 is relatively smaller than those reported in cuprates [49, 50] and iron pnictides [51], but similar to that of highly disordered superconducting thin films close to the superconductor-insulator transition [52, 53]. Another spectral survey in a 40 nm ×\times 40 nm field of view shows similar behavior (Supplementary Fig. 8); an autocorrelation analysis of the gap map over this larger range yields a decay length LΔ≈58L_{\Delta} \approx58 nm (Supplementary Figure 7), which is consistent with the expectation for the spatial variation of superconducting order parameter (Supplementary Note 7) according to the in-plane superconducting coherence length ξab\xi_{ab} (≈28\approx28-41 nm) attained from vortex imaging and analysis of the upper critical fields (Supplementary Note 3 and Supplementary Figure 7).

Two interconnected length scales for a spatially inhomogeneous superconducting state

Supplementary Figure 7. Two interconnected length scales for a spatially inhomogeneous superconducting state. a, Topographic image of a 500 nm ×\times 500 nm Sb surface with sparse Cs atoms. b, Corresponding superconducting gap map. c, Azimuthally averaged autocorrelation coefficients of the gap map (green circles), exhibiting an exponential decay characterized by a length scale LΔ≈58L_{\Delta} \approx58 nm (orange line). d, Zero-bias dI/dVdI/dV conductance map with an out-of-plane magnetic field of 0.15 T, showing a superconducting vortex. e, dI/dVdI/dV line-profile along the pink arrow in d. The flat DOS inside the gap without well-defined Caroli-de Gennes-Matricon vortex states indicates the presence of strong scattering in these crystals. f, Exponential fit to the zero-energy DOS distribution around the vortex (azimuthally averaged), yielding a coherence length of ξ≈41.1\xi\approx41.1 nm.

Notably, local spectra with a larger gap consistently exhibit higher coherence peaks and a deeper zero-bias suppression (Fig. 3i and j), implying a strong positive correlation (αc≈0.8\alpha_c \approx0.8) between Δ(r)\Delta(r) and H(r)H(r). This correlation explicitly suggests that the gap filling and smearing out of coherence peaks are due to pair-breaking scattering [54], which in turn leads to a reduction of Δ\Delta through Δ=V∑k⟨ck†c−k†⟩\Delta= V\sum_k\langle c^\dagger_k c^\dagger_{-k}\rangle as in the framework of the Bogoliubov–de Gennes theory. Consistently, local spectral fitting using the Dynes formula N(E)=Re[(E−iΓ)/(E−iΓ)2−Δ(θ)2]N(E) = Re[(E - i\Gamma)/\sqrt{(E - i\Gamma)^2 - \Delta(\theta)^2}] reveals that the extracted pair-breaking parameter Γ(r)\Gamma(r) is anti-correlated with Δ(r)\Delta(r) (Supplementary Fig. 8h-k), further supporting that the gap inhomogeneity is closely associated with spatially inhomogeneous pair breaking. Overall, the observation of microscopic inhomogeneity at the lowest TT complements to the percolative superconducting transition (stemming from a distribution of TcT_c), consistently establishing a full picture of spatially heterogeneous superconductivity in these samples.

What could be the potential origin of such an inhomogeneity? First, the influence of local strains and surface Cs concentrations can be precluded (Supplementary Notes 9 and 10). Moreover, the crosscorrelation between the position of Sn dopants and Δ(r)\Delta(r) is almost zero (Fig. 3h and Supplementary Fig. 8 for more datasets), suggesting that the inhomogeneity is not inherited from the distribution of dopants. This is further verified by a systematic comparison of the gap distribution across different Sn doping levels (Supplementary Note 11): The normalized gap variation σ/Δˉ\sigma/\bar{\Delta} remains small for x=0.06x = 0.06, 0.120.12 and 0.300.30 with values of 0.0120.012, 0.0100.010 and 0.0200.020, respectively, whereas it reaches 0.0510.051 in the stripe-ordered x=0.09x = 0.09 sample (Supplementary Table S2). The x=0.30x = 0.30 sample indeed exhibits noticeable spatial variations in its normal-state DOS, yet its superconducting gap remains rather homogeneous (Supplementary Fig. 13). Given that remarkable inhomogeneity of Δ\Delta is absent in both phase regions I and III in the TT-xx phase diagram displayed in Figure 1 (for pristine CsV3_3Sb5_5 σ/Δˉ≈0.018\sigma/\bar{\Delta} \approx0.018, [55]), we conclude that it is most likely linked to the occurrence of the unidirectional band folding from short-ranged charge-stripe order in phase II (Supplementary Fig. 15), as further discussed below.

Normal fluids in the superconducting state

Besides the spatially varying superconducting gap, superconductivity in stripe-ordered samples (x=0.07x = 0.07 and 0.090.09) in the phase region II is also distinguished by the presence of copious low-energy quasiparticle excitations at temperatures far below TcT_{\mathrm{c}}. The first implication comes from specific heat study. In Figure 4a we present the electronic specific heat Ce(T)C_{\mathrm{e}}(T) of CsV3_3Sb4.91_{4.91}Sn0.09_{0.09} obtained after subtraction of the phonon contribution and nuclear Schottky term (Methods and Supplementary Fig. 17). Below TcsT_{\mathrm{c}}^{\mathrm{s}}, Ce/TC_{\mathrm{e}}/T develops an extremely broadened anomaly with a heavily suppressed jump height (ΔCe/γnTc≈0.43\Delta C_{\mathrm{e}}/\gamma_{\mathrm{n}}T_{\mathrm{c}} \approx0.43 compared to the BCS value of 1.431.43), reflecting a substantial distribution of local TcT_{\mathrm{c}}. The low-TT (<0.7< 0.7 K) profile can be fitted to Ce/T=γ0+a′T−5/2exp⁡[−Δ(0)/kBT]C_{\mathrm{e}}/T = \gamma_{0} + a'T^{-5/2}\exp[-\Delta(0)/k_{\mathrm{B}}T] [56] with γ0≈11.7\gamma_{0} \approx11.7 mJ mol−1^{-1} K−1^{-1} and Δ(0)=0.27\Delta(0) = 0.27 meV; here a′a' is a constant and kBk_{\mathrm{B}} is the Boltzmann constant. Such behavior provides two important insights: First, the specific heat of superconducting electrons takes the form suggestive of a fully gapped pairing state [detailed analysis of Ce(T)C_{\mathrm{e}}(T) is presented in Supplementary Note 13, where we verifie the validity of two-band and (modified) single-band BCS α\alpha-model for x≤0.06x \le0.06 and x≥0.07x \ge0.07, respectively]. Second, a large residual linear term γ0T\gamma_{0}T with γ0/γn≈38%\gamma_{0}/\gamma_{\mathrm{n}} \approx38\% (γn≈31.0\gamma_{\mathrm{n}} \approx31.0 mJ mol−1^{-1} K−1^{-1} is the normal-state Sommerfeld coefficient, Figure 4a) is necessarily introduced to trace the leveling off Ce/TC_{\mathrm{e}}/T at the lowest TT that guarantees the entropy balance condition (Supplementary Note 13 and Supplementary Fig. 18); it presumably arises from gapless quasiparticles at the chemical potential that do not superconduct down to at least 0.10.1 K --- straightforwardly, it means more than one third of conduction electrons stay unpaired at T/Tc≈0.05T/T_{\mathrm{c}} \approx0.05, constituting a prominent branch of normal fluid in the superconducting state. Indeed, the presence of an abundant normal fluid is another unique feature of superconductivity in the charge-stripe phase region II as demonstrated in Figure 4b: γ0/γn\gamma_{0}/\gamma_{\mathrm{n}} is remarkably enhanced for x=0.07x = 0.07 and 0.090.09 (strikingly reaching ∼63%\sim63\% in the former), whilst stays relatively low for x=0x = 0, 0.060.06, 0.120.12 and 0.300.30 (these residual terms may not be intrinsic; see Supplementary Note 13).

Residual normal fluid in CsV3Sb4.91Sn0.09

Figure 4. a, The electronic specific heat Ce(T)/TC_{\mathrm{e}}(T)/T of CsV3_3Sb4.91_{4.91}Sn0.09_{0.09} (blue circles) with the Schottky anomaly (navy dashed line) subtracted from data of C(T)−Cph(T)C(T)-C_{\mathrm{ph}}(T) (cyan symbols, see Methods for details). Orange line indicates a BCS ss-wave fit with a residual linear term γ0\gamma_0: Ce/T=γ0+a′T−5/2exp⁡[−Δ(0)/kBT]C_{\mathrm{e}}/T = \gamma_0 + a'T^{-5/2}\exp[-\Delta(0)/k_{\mathrm{B}}T]. Horizontal dashed line indicates the normal-state Sommerfeld coefficient γn\gamma_{\mathrm{n}}. b, γn\gamma_{\mathrm{n}} (blue diamonds) and γ0\gamma_0 (olive circles) plotted against Sn doping level xx. Background colours differentiate phase regimes. c, Superconducting spectra for x=0x = 0 [58] (blue), x=0.09x = 0.09 (red) and x=0.3x = 0.3 (olive). The experimental temperature is shown in units of Tc0T_{\mathrm{c0}}. d, Schematic illustration of the Fermi surface in CsV3_3Sb5−x_{5-x}Snx_x, with colour-coded arrows highlighting the dominant scattering vectors. The dashed dark lines denote the first Brillouin zone. e-h, Twofold-symmetrized quasiparticle interference patterns at several energies measured in CsV3_3Sb4.91_{4.91}Sn0.09_{0.09}: e, −5-5 meV, away from the superconducting gap; f, g, −0.32-0.32 mV and −0.24-0.24 mV, within the superconducting gap; h, 00 meV, deep inside the gap (see Method and Supplementary Note 15). The quasi-1D scattering event labelled as q1q_1 persists to zero energy even at the lowest temperature. STM setups: c. Vs=1.2V_{\mathrm{s}} = 1.2 mV, It=0.15I_{\mathrm{t}} = 0.15 nA, Vm=30V_{\mathrm{m}} = 30 µV for x=0x = 0; Vs=−1V_{\mathrm{s}} = -1 mV, It=0.6I_{\mathrm{t}} = 0.6 nA, Vm=10V_{\mathrm{m}} = 10 µV for x=0.09x = 0.09; Vs=2V_{\mathrm{s}} = 2 mV, It=1I_{\mathrm{t}} = 1 nA, Vm=40V_{\mathrm{m}} = 40 µV. e, Vs=−5V_{\mathrm{s}} = -5 mV, It=1I_{\mathrm{t}} = 1 nA, Vm=2V_{\mathrm{m}} = 2 mV; f-h. Vs=−2V_{\mathrm{s}} = -2 mV, It=0.5I_{\mathrm{t}} = 0.5 nA, Vm=50V_{\mathrm{m}} = 50 µV.

The concurrence of a full superconducting gap and profuse quasiparticle DOS at the Fermi level (EFE_{\mathrm{F}}) can originate from either phase separation (with a large fraction of the sample being nonsuperconducting), or a strong pair-breaking effect triggered by a specific scattering process [32, 57]; the latter, under the condition of weak, nonmagnetic disorder [33], has been established as a hallmark of unconventional superconductivity possessing sign-reversal order parameters [34, 36, 37, 58, 59]. Our STM results unequivocally nail down the pair-breaking origin of the normal fluid. Figure 4c shows a direct comparison of the superconducting spectra for x=0x = 0 [60], 0.090.09 and 0.30.3, acquired at temperatures of 0.015Tc00.015T_{\mathrm{c}0}, 0.01Tc00.01T_{\mathrm{c}0} and 0.09Tc00.09T_{\mathrm{c}0}, respectively. Only the composition x=0.09x = 0.09 in phase region II exhibits a prominent residual DOS (approximately 30%30\% of the normal-state DOS) at zero energy down to lowest TT; at x=0.3x=0.3, a large, U-shaped gap with negligible in-gap DOS emerges. This trend is in excellent agreement with the specific heat data.

Further elucidation of the momentum-space origin of the residual in-gap DOS comes from quasiparticle interference imaging. As sketched in Figure 4d, the salient scattering channels of the normal state include intra-pp-orbital scattering (q0\mathbf{q}_0), scattering of the quasi-1D segments of the kagome dd-band (q1\mathbf{q}_1), and scattering between the arcs of triangular pockets (q2\mathbf{q}_2). The one-of-a-kind scattering element in phase region II is the unidirectional, quasi-1D stripe features (labeled as q′\mathbf{q}' and q′′\mathbf{q}'') that span almost the entire Brillouin zone (Figure 4e); these features may rise from the scattering between the original quasi-1D bands and their folded replicas owing to the formation of single-QQ stripelike CDW (Supplementary Figure 15) [30]. Upon entering the superconducting gap, most of the scattering events fade away owing to the depletion of quasiparticles by gap opening; the prominent feature at q1\mathbf{q}_1, however, persists down to zero-energy even at 20 mK. These unidirectional signals unveil the momentum origin of the residual DOS at EFE_{\mathrm{F}}; that is, these unpaired quasiparticles mainly reside on the quasi-1D bands which are involved in the band folding corresponding to the stripelike CDW (Figure 4e and Figure 4h; Supplementary Figure 15). Moreover, the same stripe-related electronic band reconstruction is also connected to the real-space gap inhomogeneity; our spatial-resolved analyses reveal that the gap distribution Δ(r)\Delta(\mathbf{r}) (while is anti-correlated with Γ\Gamma, Supplementary Note 8) correlates positively with the stripe-induced folded-band QPI intensities, i.e., regions with larger Δ\Delta exhibit stronger features at q′\mathbf{q}' and q′′\mathbf{q}'' (Supplementary Note 12). This immediately rules out a straightforward competition between the stripelike CDW and superconductivity; instead, it implies that the heterogeneous superconductivity is tied to both charge-stripe-related electronic structure and spatial dependent pair-breaking effect. A most likely scenario is thus the short-range stripelike CDW imposes a strong pair-breaking scattering effect upon the superconducting state, consequently engenders the spatially varying order parameter and sizeable normal fluid DOS [32], as have been established in the cases of dd-wave superconductors [36, 37].

Charge-stripe order revealed by QPI images

Supplementary Figure 15. Charge-stripe order revealed by QPI images. a, Schematic illustration of the Fermi surface of CsV3Sb5−xSnx\mathrm{CsV_3Sb_{5-x}Sn_x}. The color-coded arrows denote the main scattering vectors. b, Schematic of the stripe order, with a unidirectional periodicity of approximately 3a03a_0. c, Band folding induced by the charge stripe order: the quasi-1D bands (shown in red) are folded along the Γ\Gamma–M direction (dashed black arrow), giving rise to two new scattering vectors q′q^\prime and q′′q^{\prime\prime}. d, Real-space visualization of short-range stripe order in strained x=0.09x = 0.09 sample. Upper panel: dI/dV\mathrm{d}I/\mathrm{d}V map showing the short-range modulations (marked by black arrows); lower panel: line-profile along the dashed green line, revealing a periodic modulation of approximately 3a03a_0. e-h, QPI images at high energies for x=0.06x = 0.06 (e), 0.090.09 (f), 0.120.12 (g) and 0.30.3 (h). The unique scattering wavevectors of q′q^\prime and q′′q^{\prime\prime} can only be observed in the x=0.09x = 0.09 samples.

Discussion

A distinct heterogeneous superconducting state that develops peculiarly in the charge-stripe phase regime (II) of CsV3Sb5−xSnx\mathrm{CsV_3Sb_{5-x}Sn_x} (Figure 1b and Figure 1c) has been uncovered by our multimodal investigations. It cannot be simply attributed to the inhomogeneity of dopant distribution or local strain fields, nor a simple competition between the charge order and superconductivity. This state, unforeseen in a three-dimensional (3D) weakly-correlated system and has been overlooked thus far in the study of AV3Sb5AV_3\mathrm{Sb}_5 series, adds vigorously to the rich emergent physics in kagome lattice superconductors [61, 62]. We emphasize that our results can hardly be reconciled with the sign-invariant ss-wave pairing for the following reasons. (i) Sn substitution only introduces nonmagnetic scattering centers [30], thus, Anderson’s theorem [33] should be complied with. (ii) Accordingly, BCS-type superconductivity is insensitive to impurity scattering up to a substantial strength of disorder potential [33, 58], which suffices to bring the system close to the mobility edge [63]; whilst spatially inhomogeneous superconductivity naturally sets in [63, 64] at such high levels of disorder, there is compelling evidence that our 3D crystals are far from the localization threshold on the metallic side (Supplementary Note 14). (iii) STM results indicate that the pair breaking is more likely caused by scattering off the disorder potential associated with the short-range CDW (Supplementary Note 15), as evidenced by the remnant quasiparticle DOS pertains to the Fermi sheets participating in the charge-stripe-induced unidirectional band folding (Figure 4h); in contrast, conventional ss-wave pairing is known to be robust against this sort of perturbation [6, 65].

In essence, all our major discoveries, i.e., (1) the percolative superconducting precursor, (2) spatially-varying superconducting order parameter on a length scale of the order of ξab\xi_{ab} and (3) the residual normal fluid concentrated on specific Fermi surfaces, are consistent with the phenomenology that a sign-changing unconventional superconducting phase is exposed to strong pair-breaking effect which has been widely investigated on the background high-TcT_c cuprates [32, 66, 67]: scattering between momentum-space regions with opposite signs of superconducting order parameter is particularly effective in destroying the coherent superconducting order, engendering a spontaneous tendency toward heterogeneity. The resulted superconducting state exhibits inherent spatially nonuniform signatures (that can be unrelated to the distribution of disorder) and incorporates a remarkable density of gapless, unpaired quasiparticles [32], in agreement with both our experimental observations and earlier results in overdoped cuprates [34, 35, 36, 37]. As such, we have managed to provide strong evidence for the occurrence of sign-reversal superconductivity in the kagome Cs135 family (CsV3_3Sb5_5 and its doped derivatives). We also note that the pair-breaking scattering in CsV3_3Sb5−x_{5-x}Snx_x is predominantly attributed to the short-range stripelike CDW whose correlation length is putatively comparable to ξab\xi_{ab} [67] (Supplementary Note 15), instead of the point-like impurities as the case in cuprates [32, 37]. The evolution of the vortex-core spectra is also consistent with this interpretation. The zero-energy conductance peak observed in the vortex cores at x=0x = 0 [16] becomes broadened and disappears as the short-range stripe-like CDW develops in phase region II, leaving a featureless, normal-state-like spectrum (Supplementary Fig. 7). By contrast, finite-energy conductance peaks reappear at x=0.3x = 0.3, where the stripe-like CDW is weak or no longer discernible (Supplementary Fig. 13).

Thanks to the unique quantum interference between the electron wavefunctions of three sublattices in the geometrically frustrated kagome lattice, diverse theoretical proposals of sign-reversal pairing states have been raised for kagome superconductors; these includes (p+ip)(p+ip)-wave (Figure 5a), (d+id)(d+id)-wave (Figure 5b), ff-wave (Figure 5c) and s+−s^{+-} states (Figure 5d) [68, 69, 70, 71] as well as exotic PDW order [72]. Despite that the exact pairing symmetry cannot be conclusively determined at this stage, we suggest that the singlet d+idd+id (chiral dd) [68, 69, 71] and s+−s^{+-} [70, 71] pairing states are more promising candidates, both of which can give rise to the unidirectional pair-breaking scattering observed in the STM measurements (at present, the QPI analysis cannot give a more definitive identification of the pairing symmetry, see Supplementary Note 17). On the other hand, the nodal ff-wave pairing (Figure 5c) can be generally ruled out as there is no evidence for gap nodes in our specific heat (Supplementary Note 13) and STM data (Supplementary Note 16); the p+ipp+ip state (Figure 5a) is also less likely due to the absence of strong pair breaking effect of Sn dopants that is promised for spin-triplet pairing (Supplementary Note 17). Moreover, the unusual superconducting state in CsV3_3Sb5−x_{5-x}Snx_x (x=0.09x = 0.09) can hardly be associated with the PDW state, since the spatial modulation of the superconducting order parameter lacks the periodicity featuring a PDW order (Figure 5e-Figure 5h). Several important implications of our results deserve to be stressed: Heterogeneous unconventional superconductivity emerges only in the charge-stripe phase regime where the unidirectional band folding can be identified (Figure 1), which highlights the strikingly intricate correspondence between CDW and superconductivity in the Cs135 family [73, 74]. The effective pair breaking promoted by an extend CDW-related disorder potential may indicate distinct responses to disorder for unconventional kagome superconductors [75]. The persistent gapless feature of the Fermi sheet participating in the unidirectional folding of charge stripes (Figure 4h) provides crucial information about the possible location of sign reversal of the superconducting order parameter (Supplementary Note 17). Our work thus identifies charge-stripe-ordered CsV3Sb5−xSnx\mathrm{CsV_3Sb_{5-x}Sn_x} as a privileged platform for the exploration of emergent unconventional superconductivity and its interplay with coexisting electronic orders. Future phase-sensitive probes and theoretical efforts may help to pinpoint the exact symmetry of superconducting order parameter and the microscopic mechanisms for the occurrence of heterogeneous superconductivity.

Possible sign-reversal pairing states and the absence of PDW state

Figure 5. Possible sign-reversal pairing states and the absence of PDW state. a–d, Illustrations of four representative sign-reversal pairing states: a, chiral p-wave (p+i**p); b, chiral d-wave (d+i**d); c, f-wave; d, s±_{\pm} wave. Colours in a and b indicate the phase of superconducting order parameter, which varies as a function of the polar angle φ\varphi (inset of a). In c and d, red and blue colours denote the positive and negative sign of superconducting order parameter, respectively, with their darkness implying the gap amplitude. The dashed hexagons mark the boundary of the first Brillouin zone; coloured hexagon and circle rings represent the Fermi surface contributed by the vanadium (kagome) d-orbitals and Sb p-orbitals, respectively. Black arrows denote scattering processes that preserve the superconducting order, whereas red arrows indicate scattering events potentially cause breaking of Cooper pairs. The two quasi-1D bands (blue) in d are folded d-electron bands induced by the charge-stripe order. e, Gap map with higher spatial resolution of a 20 nm × 20 nm region of x=0.09x = 0.09, showing no signature of PDW state. f–h, Left panel: dI/dV\mathrm{d}I/\mathrm{d}V linecuts along three different lattice directions (arrows in e, black, ochre and cyan for f, g and h, respectively); right panel: corresponding gap variation, both show absence of discernible periodic modulation.

Methods

Single crystal growth and characterizations

Single crystals of CsV3Sb5−xSnx\mathrm{CsV_3Sb_{5-x}Sn_x} were synthesized via a self-flux growth method from a mixture of Cs2Sb3\mathrm{Cs_2Sb_3}, VSb2\mathrm{VSb_2} and SnSb\mathrm{SnSb}. The mixture was sealed in an evacuated quartz ampoule and heated at 1000 °C for 30 h, followed by cooling at a rate of 2 °C/h down to 700 °C. The platelike as-grown CsV3Sb5−xSnx\mathrm{CsV_3Sb_{5-x}Sn_x} single crystals with typical sizes of 5×5×0.15 \times5 \times0.1 mm3^3 are stable in air. X-ray diffraction (XRD) measurement demonstrated their [00ll] orientation; in this work, we define the cc axis along the crystallographic [1] direction and the abab plane perpendicular to it. Chemical compositions were determined by energy-dispersive X-ray spectroscopy (EDS) and have been further verified by STM topographic images (Supplementary Note 1).

Transport measurements

Electrical resistivity measurements were performed in a Quantum Design Dynacool-14 T physical property measurement system (PPMS) equipped with a dilution refrigerator. Single crystals of CsV3Sb5−xSnx\mathrm{CsV_3Sb_{5-x}Sn_x} were cut into rectangular bar shapes. Electrical contacts were made by attaching platinum wires to the (001) surface of the sample in a conventional four-lead configuration using silver paste (DuPont 4929N). For the x=0.07x = 0.07 and 0.09 samples, the zero-field paraconductivity Δσ(T)\Delta\sigma(T) is defined as: Δσ(T)=σ(T)−σn(T)=1/ρ(T)−1/ρn(T)\Delta\sigma(T) = \sigma(T)-\sigma_n(T) = 1/\rho(T) - 1/\rho_n(T), where the normal-state resistivity ρn(T)\rho_n(T) was obtained by fitting to the form ρn(T)=ρ0+A2T2+A5T5\rho_n(T) = \rho_0+A_2T^2+A_5T^5 (ρ0\rho_0, A2A_2 and A5A_5 are fitting parameters).

Magnetization measurements and torque magnetometry

The dc magnetization was measured down to 0.4 K using a Quantum Design magnetic property measurement system (MPMS) equipped with a helium-3 (3^3He) insert. The diamagnetic responses of samples were tracked in both zero-field-cool (ZFC) and field-cool (FC) processes, under a constant external field H=5H = 5 Oe applied parallel to the cc axis. The magnetic susceptibility χ\chi was calculated considering the demagnetizating factors given by the sample geometries.

Measurement of the magnetic torque τ(H)\tau(H) were performed using the method of piezoelectric torque magnetometry. A small piece of single crystal was attached to the tip of a piezoresistive cantilevers (SCL Sensortech PRSA-L300), which was mounted to a 3^3He probe and loaded into a Quantum Design PPMS. In practice, the resistance of SCL sensor (essentially reflecting the voltage drop across a built-in Wheatstone bridge) was measured and converted to the magnetic torque: τ∝R(H)−R(H=0)\tau\propto R(H) - R(H = 0). The transverse magnetization M⊥M_\perp was derived as M⊥=τ/μ0HM_\perp= \tau/\mu_0H.

Effective-medium model for the percolation process

The putative percolation process above the bulk TcT_c can be properly described within the effective-medium theory (EMT) [75, 76], which has been frequently exploited in the analysis of spatially inhomogeneous superconductors (e.g. high-TcT_c cuprates [42, 43] and oxide heterointerfaces [48, 76]) in a certain temperature range above TcT_c. Within this picture, the systems comprise a mostly random network of superconducting and metallic regions; accordingly, Tc0T_{c0} marks the temperature at which the fraction PP of superconducting clusters reaches a threshold PπP_{\pi} that renders a fully-connected superconducting path across the sample. Here, we chose a 3D nearest-neighbor site percolation model [43, 77, 78] for EMT analysis. Such a model treats the sample as an ensemble of well-connected small cubic grains, each having a local TcT_c; with decreasing TT, the fraction of superconducting grains grows, eventually percolates at T=TπT = T_{\pi} where PP adopts a critical value Pπ≈0.31P_{\pi} \approx0.31 [41, 42]. The resistivity of an individual grain is set to a universal value RnR_n above its local TcT_c and a vanishingly small R0=10−4RnR_0=10^{-4}R_n below it. Thereby, the spatial inhomogeneity stems only from the distribution of local TcT_c that is depicted by a function g(T)g(T). The TT dependence of superconducting fraction PP is thus:

P(T)=∫T∞g(T′) dT′(1)P(T) = \int_T^{\infty} g(T')\,\mathrm{d}T' \tag*{(1)}

To delineate the drastic enhancement of PP when TT approaches TcST_c^S (presumably due to proximity effect [33]), we opted for a two-component form of g(T)g(T): g=ug1(T)+(1−u)g2(T)g = u g_1(T)+(1-u)g_2(T); uu is a weighing factor, g1g_1, g2g_2 are two Gaussian distribution functions with the same mathematic expectation T0T_0 and half-width-at-half-maximum (HWHM) Ξ1\Xi_1 and Ξ2\Xi_2, respectively (Ξ1>Ξ2\Xi_1 > \Xi_2, see Supplementary Figure 5). Above a critical temperature TπT_{\pi} [P(Tπ)=Pπ=0.31P(T_{\pi}) = P_{\pi} = 0.31], the profile of dc conductivity σ(T)=1/ρ(T)\sigma(T) = 1/\rho(T) follows a trend given by the EMT:

σ−(1−P+P/R0)1−P+P/R0+(1/Pπ−1)σP+σ−1/R0P+(1−P)/R0+(1/Pπ−1)σ(1−P)=0(2)\frac{\sigma- (1-P+P/R_0)}{1-P+P/R_0+(1/P_{\pi}-1)\sigma}P+\frac{\sigma- 1/R_0}{P+(1-P)/R_0+(1/P_{\pi}-1)\sigma}(1-P)=0 \tag*{(2)}

As demonstrated by the fitting curves in Figs. 2a and c, this EMT modeling provides a reasonable description of the experimental paraconductivity data for the x=0.07x=0.07 and 0.090.09 samples (in a temperature range of ∼\sim1.4-3.6 K and ∼\sim2.1-3.5 K, respectively). In particular, the exponential attenuation upon warming is reproduced by fits to Eq. (2). We suggest that such a percolation scenario, in spite of its oversimplification, captures some of the main characters of emerging superconductivity precursor above bulk TcT_c in these samples. It should be noticed that our samples lack the inherit normal-state inhomogeneity (Supplementary Note 1 and Supplementary Fig. 2) that prevails in cuprates due to heterogeneous charge localization [79]; the percolative model instead reflects an unusual interplay between stripelike CDW and superconductivity in CsV3_3Sb5−x_{5-x}Snx_x.

Measurement and analysis of specific heat

Specific heat of CsV3_3Sb5−x_{5-x}Snx_x was measured down to 0.1 K in a Dynacool-14T PPMS equipped with a dilution refrigerator and 3{}^3He system. During the measurements, the temperature rise in each relaxation cycle was kept at ΔT/T=3%\Delta T/T = 3\%. In our samples, C(T)C(T) incorporates contributions from electrons (CeC_e), phonons (CphC_{ph}) and the Schottky anomaly of nuclear spins (CSchC_{Sch}). The electronic contribution CeC_e was obtained by subtracting CphC_{ph} and CSchC_{Sch} from the raw data. At low TT, the phonon contribution takes the form Cph=βT3+ηT5C_{ph}=\beta T^3+\eta T^5; we assumed that β\beta and η\eta are independent of HH and employed the fit C(T)=γnT+βT3+ηT5C(T)=\gamma_nT+\beta T^3+\eta T^5 [79,80] to data between 0.5 and 4 K under μ0H=3\mu_0H=3 T along cc (at which the superconductivity is fully quenched in all samples, thus Ce=γnTC_e=\gamma_nT), see Supplementary Figure 17. The value of Sommerfeld coefficient γn\gamma_n was verified by fitting the zero-field normal state C(T)C(T) to the same formula (Supplementary Figure 17), endorsing that γn\gamma_n does not vary under HH at T>TcT>T_c. The Schottky term CSchC_{Sch} is only resolvable below approximately 0.5 K; we fit it using a two-level model: CSch=Dx2ex/(1+ex)2C_{Sch}=Dx^2e^x/(1+e^x)^2 (DD is a constant, x=ΔE/kBTx=\Delta E/k_BT, ΔE\Delta E is the energy separation between two levels) [80]. It yields reasonable fitting results in a temperature range from 0.2 to 0.4 K (Figure 4a, Supplementary Figure 17).

Six-panel plots of specific heat data and fitted contributions

Supplementary Figure 17. Procedures for separating the electronic contribution CeC_{\mathrm{e}} from the raw data of C(T)C(T). a-f, Low-TT specific heat data measured in CsV3Sb5−xSnx\mathrm{CsV}_{3}\mathrm{Sb}_{5-x}\mathrm{Sn}_{x} with x=0x = 0 (a), x=0.06x = 0.06 (b), x=0.07x = 0.07 (c), x=0.09x = 0.09 (d), x=0.12x = 0.12 (e) and x=0.3x = 0.3 (f). Blue and purple circles are C/TC/T measured under zero magnetic field and μ0H=3\mu_{0}H = 3 T (H∥cH \parallel c), respectively. Royal solid line and green dashed lines are fitting curves of the phononic term (Cph/TC_{\mathrm{ph}}/T) and the nuclear Schottky term (CSch/TC_{\mathrm{Sch}}/T) as described in Methods. Red symbols denote the electronic specific heat (Ce/TC_{\mathrm{e}}/T) attained from C/T−Cph/T−CSch/TC/T - C_{\mathrm{ph}}/T - C_{\mathrm{Sch}}/T (Methods).

STM measurements

The majority of STM experiments were performed with a custom-built, dilution refrigerator-based systems with a working temperature of 20 mK at the Synergetic Extreme Condition User Facility A7 experimental station of the Institute of Physics, Chinese Academy of Sciences. Single crystals were cleaved in situ at 4.2 K under ultrahigh vacuum, then cooled to 20 mK at the STM head. PtIr tips were calibrated on polycrystalline Au prior to the measurements. Spectroscopic data were acquired using a standard lock-in technique at a frequency of 827.183 Hz with a modulation voltage of 10–50 μV. With cryogenic temperature cleaving, we were able to obtain relatively large regions with sparse Cs atoms on the surface; clean Sb surfaces were subsequently obtained by sweeping away loosely bonded Cs atoms with an STM tip (Fig. 3 and Supplementary Fig. 8). Clustering of Cs atoms on the surface might alter the local superconducting gap, but only within a spatial range of ~5 nm (Supplementary Note 10).

Signatures of the charge stripes. For x=0.07x = 0.07 and 0.090.09, the existence of short-range charge stripe is evident from the sudden appearance of q′\mathbf{q}' and q′′\mathbf{q}'' in the QPI pattern (Figure 4e): they are located at approximately 1/3 and 2/3 of (3/2)1/2QBragg(3/2)^{1/2}Q_{\mathrm{Bragg}} (along Γ\Gamma-K), and their energy dispersions are in good agreement with the quasi-1D vanadium dxz/yzd_{xz/yz} orbitals [36]; thus, a straightforward explanation is that the emergence of charge-stripe order folds the quasi-1D kagome dd-bands with a vector of roughly 1/3 along one of the three lattice directions [36]; the two new channels arise from the scattering between their original and replica bands. In fact, short-range single-QQ 3a03a_0 modulations can be directly observed in the dI/dVdI/dV maps once the surface reconstruction of Sb atoms is suppressed (Supplementary Figure 15).

Superconducting gap map. The spectra acquired at each pixel were first smoothed via a Gaussian filter and then interpolated with second-degree polynomials. The derivative of each spectrum was subsequently calculated using the central difference method, and the zero-crossings were identified as potential coherence peaks. The superconducting gap size was then defined as Δ=(Δ++Δ−)/2\Delta= (\Delta^{+} + \Delta^{-})/2.

QPI analysis. Momentum-space information of the superconducting gap function is reflected in the intensity variations in the Bogoliubov QPI maps. When the energy sweeps to inside the gap, the intensity of the intra-pp-orbital scattering (q0\mathbf{q}_0) and the intra-dd-orbital scattering (q2\mathbf{q}_2) is strongly suppressed (Figure 4 and Supplementary Figure 20). The QPI images shown in Figure 4 were 2-fold symmetrized to improve signal-to-noise. To seek possible phase-sensitive evidence for sign-changing pairing states, we performed HH-dependent and phase-referenced QPI analyses [81–84] (Supplementary Fig. 22); during the data analysis we used g(q,E)g(\mathbf{q}, E) maps instead of the Fourier transform of the conductance-ratio maps Z(r,E)=g(r,+E)/g(r,−E)Z(\mathbf{r}, E) = g(\mathbf{r}, +E)/g(\mathbf{r}, -E), because the Z(q,E)Z(\mathbf{q}, E) signals in our experiments are rather weak at low energies inside the superconducting gap (Supplementary Fig. 22j–l) and hence the ZZ-map analysis becomes less reliable. The absence of a clear phase-sensitive QPI signature does not necessarily rule out the sign-changing pairing proposed here, because the dominant observed scattering is intra-pocket and could not connect regions with opposite gap signs (see details in Supplementary Note 17).

Supplementary Fig. 20, panels a–h showing impurity states and real-space origins of q1 and q2 signals in the BQPI map

Supplementary Figure 20. Supplementary Fig. 20. Impurity state and real-space origins of q1\mathbf{q}_1 and q2\mathbf{q}_2 signals in the BQPI map. a, Zero-bias dI/dVdI/dV map of CsV3_3Sb4.91_{4.91}Sn0.09_{0.09} (Figure 4 of the main text). Green circles mark the positions of the V-site defects which generate in-gap impurity states, and the orange arrows mark the standing wave patterns near one of these defects. b, Spectra showing the in-gap state (red curve) measured at the red spot in a, together with the spectrum far away from the defects (blue curve). c, The FT of a, showing two dominant sets of scattering vectors: q1\mathbf{q}_1 associated with the quasi-1D bands and the arc-like q2\mathbf{q}_2 feature. Note that their orientations are different. d, FT-filter map of the q2\mathbf{q}_2 signals in c. The green circles and orange arrows are shown in the same positions as in a. e, Zero-bias dI/dVdI/dV map in which the regions showing in-gap states are masked. f, FT of e, where the q2\mathbf{q}_2 signal is significantly suppressed after masking. g, Spatial distribution of Sn dopants in the same FOV as a. h, FT-filter map of the q1\mathbf{q}_1 signals in c, showing negligible correlation with the Sn distribution in g.

Impurity states. While no clear in-gap state is observed near the Sn dopants, we found that some instinct defects at the vanadium site are strong pair breakers and induce pronounced in-gap bound states near EFE_{\mathrm{F}}. Corresponding local oscillations give rise to an enhanced intensity at q2\mathbf{q}_2 in the Fourier transformations. These impurity states are spatially confined to the defect sites, in sharp contrast to the scattering events at q1\mathbf{q}_1 that is more extended in real space (Supplementary Note 15).

Data availability

The primary data underlying all the plots within the main text, as well as the supplementary resistivity, magnetization, magnetic torque and specific heat data that support the findings of this study, have been deposited in the Figshare database under DOI 10.6084/m9.figshare.34332690, see ref. [85]. Other source data generated in this study are available from the corresponding authors upon request.

Acknowledgements

We thank Zi-Xiang Li, Kun Jiang, Yi Zhou, Hong Yao, Qianghua Wang, Ziqiang Wang, Haiwen Liu and Andreas Kreisel for insightful discussions. A portion of experimental work was carried out at the Synergetic Extreme Condition User Facility (SECUF, https://cstr.cn/31123.02.SECUF).

Funding

This work was financially supported by the National Natural Science Foundation of China (Grants Nos. 12488201, 12274390 and 52261135638), the National Key Projects for Research and Development of China (Grant No. 2022YFA1602602), the Quantum Science and Technology-National Science and Technology Major Project (Grant No. 2021ZD0302802), the Basic Research Program of the Chinese Academy of Sciences Based on Major Scientific Infrastructures (No. JZHKYPT-2021-08) and the Fundamental Research Funds for the Central Universities No. WK2030000111.

Author contributions

Z.X., Zhenyu Wang and X.C. supervised the project and designed the experiments. Hongyu Li, H.R. and T.W. prepared the samples. Hongyu Li and Z.X. performed the electrical transport, magnetic torque and specific heat measurements and analyzed the data with help from X.Z., Houpu Li and Z.G. S.Y. and Zhenyu Wang conducted the STM measurements and analyzed the data with assistance from Zhuying Wang, Y.Z., X.Y. and R.W. Hongyu Li, Z.X., S.Y. and Zhenyu Wang wrote the paper with input from all authors.

Competing interests

The authors declare no competing interests.

Percolative superconducting precursors in charge-stripe-ordered CsV3Sb5-xSnx

Figure 2. Percolative superconducting precursors in charge-stripe-ordered CsV3_3Sb5−x_{5-x}Snx_x. a-d, In-plane paraconductivity Δσxx\Delta\sigma_{xx} (a and c) and ZFC susceptibility χ\chi (b and d, same data as presented in Figure 1h and Figure 1k, respectively), measured in CsV3_3Sb4.93_{4.93}Sn0.07_{0.07} (a and b) and CsV3_3Sb4.91_{4.91}Sn0.09_{0.09} (c and d). Data are displayed as hollow symbols in logarithmic scales. Orange and red solid lines are simulations based on the 3D Gaussian-type fluctuations and phase fluctuations, respectively (Supplementary Notes 3 and 4). Blue lines in a and c represent the fits of Δσxx\Delta\sigma_{xx} to the EMT model (with a two-component distribution of TcT_\mathrm{c}, see Methods and Supplementary Note 5). Dashed lines in b and d guide the eyes. Black arrows indicate characteristic temperatures Tc0T_{\mathrm{c0}}, TcsT_\mathrm{c}^{\mathrm{s}} and TdT_\mathrm{d}. e, f, A contrast between the transverse magnetization M⊥M_\perp (e) derived from torque magnetometry (Methods) and ρxx\rho_{xx} (f) measured in a CsV3_3Sb4.91_{4.91}Sn0.09_{0.09} sample under in-plane HH at different temperatures (olive, T=0.4T = 0.4 K; orange, 1.4 K; red, 2.4 K). Inset of e displays the full hysteresis loops of M⊥M_\perp. Vertical dashed lines mark the onset fields of zero resistivity. g-i, Schematic representations of the percolation process which is partially captured by the EMT approach. With decreasing TT, gradual emergence of superconducting grains (dark purple) from the metallic surroundings (light cyan) gives rise to detectable signals of diamagnetism below TdT_\mathrm{d} (g); the superconducting grains are substantially enlarged due to proximity effect when TT approaches TcsT_\mathrm{c}^{\mathrm{s}} (h) and a percolation path across the sample appears at T=Tc0T = T_{\mathrm{c0}} (i).

Spatial inhomogeneity of superconductivity in CsV3Sb4.91Sn0.09

Figure 3. Spatial inhomogeneity of superconductivity in CsV3Sb4.91Sn0.09\mathrm{CsV}_{3}\mathrm{Sb}_{4.91}\mathrm{Sn}_{0.09}. a-f, Topologic and spectroscopic characteristics in a 70 nm ×\times 10 nm field of view, including topographic image (a), dopant distribution (b), integrated DOS between ±\pm 6 meV (c) and ±\pm 50 meV (d), superconducting gap map (e) and gap-depth map (f). g, Histogram showing the distribution of the gap amplitude in e. h, Cross-correlation coefficients between the gap map versus impurity distribution (blue), integrated DOSs of ±\pm6 meV (green) and ±\pm50 meV (orange), and the gap-depth map (red). i, dI/dVdI/dV linecut along the purple arrow in a, showing the spatial variation in the superconducting gap. j, Representative spectra averaged over three different regions marked in i. k, gap amplitude (upper panel), integrated DOS between ±\pm 6 meV (middle panel) and ±\pm 50 meV (bottom panel) extracted from the linecut of i, in which the shaded regions indicate the standard deviation. l, gap depth (HH) versus gap amplitude (Δ\Delta) obtained from the line-profiled spectra, showing a positive correlation. STM setups: a. Vs=−90V_{\mathrm{s}} = -90 mV, It=0.5I_{\mathrm{t}} = 0.5 nA; c, d, Vs=−90V_{\mathrm{s}} = -90 mV, It=1I_{\mathrm{t}} = 1 nA, Vm=2V_{\mathrm{m}} = 2 mV; e, f, Vs=−1V_{\mathrm{s}} = -1 mV, It=0.6I_{\mathrm{t}} = 0.6 nA, Vm=20V_{\mathrm{m}} = 20 μ\muV; i, j, Vs=−1V_{\mathrm{s}} = -1 mV, It=0.6I_{\mathrm{t}} = 0.6 nA, Vm=20V_{\mathrm{m}} = 20 μ\muV.

This PDF File includes:

Supplementary Note 1: Determination of Sn doping level xx and local dopant concentration

Supplementary Note 2: CDW transitions in CsV3Sb5−xSnx\mathrm{CsV}_{3}\mathrm{Sb}_{5-x}\mathrm{Sn}_{x} observed by means of resistivity

Supplementary Note 3: Upper critical fields and superconducting coherence lengths

Supplementary Note 4: The contribution of superconducting fluctuations

Supplementary Note 5: Additional information about the EMT model

Supplementary Note 6: Determination of superconducting gap size from STM spectra

Supplementary Note 7: Characteristic length of the spatial inhomogeneity of superconductivity at x=0.09x = 0.09

Supplementary Note 8: Spatially inhomogeneous pair breaking revealed by local tunneling spectra in x=0.09x = 0.09 sample

Supplementary Note 9: Absence of inhomogeneous strain effects in the x=0.09x = 0.09 sample

Supplementary Note 10: Influence of surface Cs clusters on the local superconducting gap

Supplementary Note 11: Doping dependence of superconducting gap inhomogeneity

Supplementary Note 12: Spatial correlation between stripe-induced folded-band QPI and superconducting gap in the x=0.09x = 0.09 sample.

Supplementary Note 13: Analysis of the specific heat

Supplementary Note 14: Absence of localization effects in CsV3Sb5−xSnx\mathrm{CsV}_{3}\mathrm{Sb}_{5-x}\mathrm{Sn}_{x}

Supplementary Note 15: Origin of pair-breaking scattering revealed by STM

Determination of Sn doping level xx and local dopant concentrations {#sec:Supplementary Note 1}

The Sn doping level xx was determined by two methods in this work, i.e., the energy-dispersive X-ray spectroscopy (EDS) measurements on single crystals and a direct counting of the number of Sn dopants within the field of view of STM. The EDS results for samples with five nominal doping levels are presented in Supplementary Table 1; the actual compositions are close to the nominal values with a spatial inhomogeneity less than 10%. For the STM-based estimation, we note that there are two types of Sb sites in the crystalline structure of CsV3_3Sb5_5: Sb1 sites in the hexagonal center of the V-kagome lattice and Sb2 site that form two honeycomb layers above and below each kagome layer (Supplementary Fig. 1a). The Sn dopant (substitutions to the Sb atoms) appears as a dark depression in the STM topographies with its center located right in the middle of six topmost Sb atoms (Supplementary Fig. 1b), indicating that the Sn dopants favour to substitute the Sb atoms in the V3_3Sb kagome plane (the Sb1 site), in agreement with previous results [1]. By counting the number of these defects in large fields of view (typically 50-nm-squares), the concentrations can be determined with high accuracy. Supplementary Fig. 1c shows the local dopant concentration counted from topographies obtained on seven samples with the nominal composition x=0.09x = 0.09; a weak spatial variation of xx among these samples is consistent with the EDS results (Supplementary Table 1), whereas the average concentration is slightly below 0.09 (x≈0.076x \approx0.076). Nevertheless, we use the nominal compositions across the manuscript since such a small deviation does not alter our conclusions.

Local Sn concentration determined from the STM images measured for CsV3Sb4.91Sn0.09

Supplementary Figure 1. Local Sn concentration determined from the STM images measured for CsV3_3Sb4.91_{4.91}Sn0.09_{0.09}. a, A schematic showing the crystal structure of CsV3_3Sb5_5 and the position of an Sn dopant. b, STM topographic image showing the Sb2 honeycomb lattice and one doped Sn atom at the Sb1 site. c, Local Sn concentrations determined by counting the Sn atoms in different regions of seven CsV3_3Sb4.91_{4.91}Sn0.09_{0.09} samples. The orange solid line indicates the mean value, while the blue dashed line indicates the standard deviation, revealing minor variations.

Nominal xx0.060.070.090.120.30
area 10.05410.06870.09590.11520.311
area 20.06310.06170.08520.12060.318
area 30.06270.07990.08490.12690.287
area 40.06550.07450.09160.12600.312
area 50.05670.07170.08530.12150.287
Average0.06040.07130.08860.12200.301

Table 1. EDS results of the doping level xx of CsV3_3Sb5−x_{5-x}Snx_x with nominal x=0.06x = 0.06, 0.07, 0.09, 0.12 and 0.30. For each sample, five areas were measured, and xx was determined from the average of areas 1-5.

We further note that for a given surface region, the Sn concentration and the one-of-a-kind QPI features for the charge-stripe order have been checked before studying the superconducting state. As displayed in Supplementary Figure 2, the normal-state tunneling spectra of CsV3_3Sb4.91_{4.91}Sn0.09_{0.09} are uniform without notable spatial variation on the length scale of tens of nanometers. We conclude that the normal state can be regarded as spatially homogeneous in all our samples (including those displaying remarkable inhomogeneity in the superconducting state).

Normal-state dI/dV maps and linecut for CsV3Sb4.91Sn0.09

Figure 2 (PDF p. 25). Normal-state dII/dVV maps and linecut for CsV3_3Sb4.91_{4.91}Sn0.09_{0.09}. a-d, dII/dVV maps taken at bias voltages of -50 mV (a), -6 mV (b), 6 mV (c) and 50 mV (d) in the same 10 × 70 nm2^2 field of view shown in main text Fig. 3. e, dII/dVV profile along the purple arrow shown in a.

CDW transitions in CsV3_3Sb5−x_{5-x}Snx_x observed by means of resistivity

The transition entering the triple-QQ CDW phase manifests itself as a slope change in the temperature-dependent resistivity ρxx(T)\rho_{xx}(T), as seen on the x=0x = 0 and 0.06 curves in Supplementary Fig. 3a. Such feature vanishes once the short-range single-QQ stripelike CDW emerges upon Sn doping at x=0.07x = 0.07 [1]; nevertheless, a very broad anomaly can still be seen in the temperature derivative of resistivity, dρxx(T)/dT\mathrm{d}\rho_{xx}(T)/\mathrm{d}T, the onset of which is marked by arrows in Supplementary Fig. 3b. We identify this temperature as TCDWT_{\mathrm{CDW}} for x=0.07x = 0.07 and 0.09, as displayed in main text Figure 1. At higher xx (≥0.12\ge0.12), the anomaly in dρxx(T)/dT\mathrm{d}\rho_{xx}(T)/\mathrm{d}T cannot be resolved, implying that the stripelike CDW becomes increasingly short-ranged and may eventually develop a fluctuating nature [2]. This is underpinned by the disappearance of band-folding signatures induced by the single-QQ CDW at x≥0.12x \ge0.12 revealed by the STM measurements (see Supplementary Figure 15 and Supplementary Note 12). We stress that in the present study, all experimental fingerprints of stripelike CDW (and its impact on superconductivity) are significantly weakened at x≥0.12x \ge0.12; in this high-doping regime, the electronic structure closely resembles a pristine kagome lattice with the absence of superlattice reconstruction.

Temperature-dependent resistivity and characteristic superconducting temperatures of CsV3Sb5-xSnx

Figure 3 (PDF p. 26). TT-dependent resistivity of CsV3_3Sb5−x_{5-x}Snx_x and the characteristic temperatures of superconductivity for x=0x = 0 and 0.30. a, ρxx\rho_{xx} measured from 0.4 K to 300 K in samples with different xx. Inset displays a zoomed view of the superconducting transitions. Note that despite strongly enhanced residual resistivity (dotted lines in the inset) in the Sn-doped samples, metallic behavior persists up to x=0.30x = 0.30 (red curve). b, Temperature derivative of longitudinal resistivity, dρxx/dT\mathrm{d}\rho_{xx}/\mathrm{d}T, as a function of TT for the six compositions shown in a. Arrows indicate the onset of the anomaly manifesting the CDW transition. At x=0.12x = 0.12, this transition becomes invisible. c–e, In-plane resistivity ρxx\rho_{xx} (c), volume magnetic susceptibility χv\chi_v (d) and electronic specific heat Ce/TC_e/T (e) measured in undoped CsV3_3Sb5_5. f–h, same as c–e but for a sample of x=0.30x = 0.30. The characteristic temperatures of superconducting states, i.e., Tc0T_{c0}, TdT_d and TcsT_c^s are identical for x=0x = 0 and x=0.30x = 0.30 (vertical dashed lines). Ce/TC_e/T data in (h) may contain a small Schottky contribution at the lowest TT.

Upper critical fields and superconducting coherence lengths

The zero-temperature values of in-plane and out-of-plane coherence lengths (ξab\xi_{ab} and ξc\xi_c, respectively) can be derived from the measurement results of upper critical fields Hc2abH_{c2}^{ab} and Hc2cH_{c2}^{c}. According to the GL relations for an anisotropic three-dimensional (3D) superconductor [3], μ0Hc2c=Φ02πξab2)\mu_0 H_{c2}^{c} = \frac{\Phi_0}{2\pi\xi_{ab}^{2})}, μ0Hc2ab=Φ02πξabξc\mu_0 H_{c2}^{ab} = \frac{\Phi_0}{2\pi\xi_{ab}\xi_c} (Φ0=2.07×10−15\Phi_0 = 2.07 \times10^{-15} Wb is the superconducting magnetic flux quantum). We determined Hc2abH_{c2}^{ab} and Hc2cH_{c2}^{c} to be the HH-fields at which the resistivity reaches 50% of the normalstate value at each temperature (Supplementary Figure 4; a 5% criterion was also used for comparison). The Hc2(T)H_{c2}(T) data are generally tracked by the GL fits, μ0Hc2(T)=μ0Hc2(0)[(1−t2)/(1+t2)]\mu_{0}H_{c2}(T)=\mu_{0}H_{c2}(0)[(1-t^{2})/(1+t^{2})], where t=T/Tct=T/T_{c} (Supplementary Figure 4); the zero-TT limit was subsequently approached by extrapolating the fits to T=0T=0. Under the 50% criterion, ξab\xi_{ab} (ξc\xi_{c}) is estimated to be 27.0 (8.7) and 22.5 (3.8) nm for samples with x=0.07x=0.07 and x=0.09x=0.09, respectively. ξc\xi_{c} far exceeds the distance dd between adjacent kagome planes (d∼0.9d\sim0.9 nm [4]), corroborating the validity of our anisotropic 3D GL modeling. The values of ξab\xi_{ab} determined using the 5% criterion are 33.1 nm for x=0.07x=0.07 and 28.7 nm for x=0.09x=0.09. Furthermore, a parallel estimation of ξab≈41.1\xi_{ab}\approx41.1 nm can be extracted from an exponential fit to the zero-energy density of states (DOS) distribution around a vortex core in STM measurements, see Supplementary Note 7 and Supplementary Figure 7-Supplementary Figure 7.

Upper critical fields of CsV₃Sb₅₋ₓSnₓ for $x = 0.07$ and $0.09$

Supplementary Figure 4. Upper critical fields of CsV₃Sb₅₋ₓSnₓ (x=0.07x = 0.07 and 0.090.09). a, b, d, e, ρxx(T)\rho_{xx}(T) measured under varying magnetic fields in samples with x=0.07x = 0.07 (a and b) and x=0.09x = 0.09 (d and e), with HH applied in the abab plane (a and d) and along the cc axis (b and e), respectively. All data were measured with an applied current I=0.1I = 0.1 mA. Dashed horizontal lines denote the 50% (green) and 5% (blue) criteria (with regard to the normal-state ρxx\rho_{xx}) of determination of Hc2H_{c2}. c, f, The upper critical field Hc2(T)H_{c2}(T) for x=0.07x = 0.07 (c) and 0.090.09 (f). Symbols are values obtained using the 50% and 5% criteria. Dashed lines are trajectories predicted by the GL models.

The contribution of superconducting fluctuations

Aside from the local TcT_{c} inhomogeneity, the resistivity rounding above the superconducting transition (main text Fig. 1g and j, Supplementary Fig. 3a, inset) can potentially result from strong superconducting fluctuations [5]. Here we consider two types of fluctuations of the superconducting order parameter: (i) The Gaussian amplitude fluctuations [6] and (ii) the phase fluctuations [7]. The influence of (i) is usually analyzed in the GL scheme, with the corrections to the normal-state kinetic characteristics described by the well-known Aslamazov-Larkin (AL) theory [6]. For an anisotropic 3D superconductor at temperatures not far above TcT_{c}, the AL expressions for fluctuating diamagnetism and paraconductivity in the weak field limit are [8, 9, 10]:

χAL≃2π23kBTcΦ02ξab2ξc(T−TcTc)−1/2(3)\chi_{\mathrm{AL}}\simeq\frac{2\pi^{2}}{3}\frac{k_{\mathrm{B}}T_{c}}{\Phi_{0}^{2}}\frac{\xi_{ab}^{2}}{\xi_{c}}\left(\frac{T-T_{c}}{T_{c}}\right)^{-1/2} \tag*{(3)}
ΔσAL≃e232ℏξc(T−TcTc)−1/2(4)\Delta\sigma_{\mathrm{AL}}\simeq\frac{e^{2}}{32\hbar\xi_{c}}\left(\frac{T-T_{c}}{T_{c}}\right)^{-1/2} \tag*{(4)}

The AL simulations displayed in main text Fig. 2 were constructed with TcT_{c} defined as TcsT_{c}^{s} and the coherence lengths (ξab,ξc\xi_{ab},\xi_{c}) using the estimations in Supplementary Note 3 (the 50% criterion).

The effect of phase fluctuations can be significant in two-dimensional (2D) superconducting systems, wherein long-range phase coherence is established at a Berezinskii-Kosterlitz-Thouless (BKT) transition occurring at TBKTT_{\mathrm{BKT}} below the mean-field TcMFT_{c}^{\mathrm{MF}} [7, 8, 11]. In bulk superconductors, phase fluctuation only becomes important when the superfluid density is low [8], or the system is close to a crossover towards Bose-Einstein condensation [10]. Considering the moderate anisotropy of Hc2H_{c2}, Γ=Hc2ab/Hc2c∼3\Gamma=H_{c2}^{ab}/H_{c2}^{c}\sim3-6, inherent phase fluctuations are unexpected in CsV3_{3}Sb5−x_{5-x}Snx_{x}. Nevertheless, we also estimated the possible contributions from this effect, whose fluctuating diamagnetism and paraconductivity are given by the Halperin-Nelson formulas [7, 11] in the weak-field limit:

χHN≃kBT2Φ02ξab2dsinh⁡2(bε)(5)\chi_{\mathrm{HN}}\simeq\frac{k_{\mathrm{B}}T}{2\Phi_{0}^{2}}\frac{\xi_{ab}^{2}}{d}\sinh^{2}\left(\frac{b}{\sqrt{\varepsilon}}\right) \tag*{(5)}
ΔσHNσn≃(2A)2sinh⁡2(bε)(6)\frac{\Delta\sigma_{\mathrm{HN}}}{\sigma_{n}}\simeq\left(\frac{2}{A}\right)^{2}\sinh^{2}\left(\frac{b}{\sqrt{\varepsilon}}\right) \tag*{(6)}

where AA is a constant with the order of unity, dd is the thickness of superconducting layer, ε=(T−TBKT)/TBKT\varepsilon= (T - T_{\mathrm{BKT}})/T_{\mathrm{BKT}}, b≃2(TcMF/TBKT−1)1/2b \simeq2(T_{\mathrm{c}}^{\mathrm{MF}}/T_{\mathrm{BKT}} - 1)^{1/2}. In practice, we took A=22.2A = 22.2, d=0.9d = 0.9 nm (spacing between adjacent kagome planes), TBKT=Tc0T_{\mathrm{BKT}} = T_{\mathrm{c0}}, TcMF=TdT_{\mathrm{c}}^{\mathrm{MF}} = T_{\mathrm{d}}. (Again, we emphasize that this modeling is completely formal and may not have a clear connection with the underlying physics in our samples.)

Simulations presented in main text Fig. 2a-d based on both the AL [Eqs. (3) and (4)] and the HN [Eqs. (5) and (6)] models fail to trace the evolution of χd\chi_{\mathrm{d}} and Δσ\Delta\sigma with increasing TT---yielding neither the correct amplitudes nor the exponential manner of decay. In high-TcT_{\mathrm{c}} cuprates where the spatial inhomogeneity has been extensively studied [12, 13, 14, 15], only the TT-dependence of the superconducting precursor deviates from Eqs. (3)-(4) with a faster suppression upon warming. Whether this is due to a percolation process [13, 14] or a short-wavelength cutoff [8, 16, 17] is debatable. In our case, however, the stark disagreement in the amplitudes effectively invalidates any interpretations referring to fluctuation. Therefore, we propose that the profound superconducting precursor effect in stripe-ordered CsV3_3Sb5−x_{5-x}Snx_x is not caused by strong superconducting fluctuations.

Additional information about the EMT model

As shown in main text Fig. 2, the two-component EMT model (Methods and Supplementary Figure 5a) yields fitting parameters for CsV3_3Sb4.93_{4.93}Sn0.07_{0.07} and CsV3_3Sb4.91_{4.91}Sn0.09_{0.09}: T0=1.3T_0 = 1.3 K, Ξ1=1.2\Xi_1 = 1.2 K, Ξ2=0.18\Xi_2 = 0.18 K, u=0.001u = 0.001 and T0=2.0T_0 = 2.0 K, Ξ1=0.65\Xi_1 = 0.65 K, Ξ2=0.2\Xi_2 = 0.2 K, u=0.01u = 0.01, respectively. Following Eq. (1) in Methods, these values yield Tπ=1.5T_{\pi} = 1.5 K for x=0.07x = 0.07 and 2.1 K for x=0.09x = 0.09. The relatively wide distribution of TcT_{\mathrm{c}}, characterized by the parameter Ξ1\Xi_1, implies a very small fraction of the sample that hosts a considerably higher TcT_{\mathrm{c}} (and presumably larger gap) than the average: As shown in Supplementary Figure 5b, the high-TT “tail” of TcT_{\mathrm{c}} distribution above the cut-off by the second, narrower distribution (with Ξ2<Ξ1\Xi_2 < \Xi_1) only contributes to about 0.1% of the total volume fraction. Obviously, such a small portion is unlikely to be captured by STM measurements. We mention that T0T_0 does not correspond to any of the observed characteristic temperatures (TdT_{\mathrm{d}}, TcST_{\mathrm{c}}^{\mathrm{S}} or Tc0T_{\mathrm{c0}}) and TπT_{\pi} is close to (but slightly higher than) Tc0T_{\mathrm{c0}}; Ξ\Xi, while it may reflect the real TcT_{\mathrm{c}} distribution to some extent, is not a specific parameter as well (Supplementary Figure 5c and Figure 5d) [14]. This notwithstanding, the EMT analysis describes the superconducting precursors in the charge-striped CsV3_3Sb5−x_{5-x}Snx_x quite satisfactorily. The proximity effect simulated by the inclusion of g2g_2 generally reproduces the abruptly boosted superconducting fraction at T≃TcST \simeq T_{\mathrm{c}}^{\mathrm{S}} (main text Figure 1h, Figure 1i, Figure 1k and Figure 1l); it engenders an expansion of superconducting clusters by bringing their surrounding metallic regions superconducting (main text Fig. 2g).

Nevertheless, our model ignores the inter-grain Josephson coupling, which may also become preponderant close to the bulk TcT_{\mathrm{c}}. Hence, the fits become less reliable in the vicinity of Tc0T_{\mathrm{c0}}. Note that the resistive tail above Tc0T_{\mathrm{c0}} (main text Figure 1g and Figure 1j) hints at a possibility that the network of clusters manifests a one-dimensional-type spatial correlation [18], in accord with the stripelike textures of charge order in the normal state.

We emphasize that the EMT does not impose strict constraints on the characteristic length scale of gap variations. The form of EMT fitting function [Eqs. (1) and (2) in Methods] does not include information about the size of superconducting patches, or grains/clusters in the 3D case. In principle, we would expect that the superconducting gap varies over a length scale set by the superconducting coherence length ξ\xi [19], as discussed in detail in Supplementary Note 7. Since the EMT analysis was performed for millimeter-sized samples, we do not see any inconsistency over these relevant length scales.

Supplementary Note 6:

Determination of superconducting gap size from STM spectra

Four-panel example of superconducting gap extraction from tunneling spectra

Supplementary Figure 6. Example of superconducting gap extraction from tunneling spectra. a, Two raw tunneling spectra with different superconducting gap sizes. b, The same spectra after Gaussian smoothing. c, Interpolated spectra obtained using second-degree polynomials. d, First-order differential of the interpolated spectra calculated by the central-difference method. The zero-crossings marked by the dashed lines identify the coherence-peak positions at Δ−\Delta^{-} and Δ+\Delta^{+}, from which the superconducting gap is defined as Δ=(Δ++Δ−)/2\Delta= (\Delta^{+} + \Delta^{-})/2.

Characteristic length of the spatial inhomogeneity of superconductivity at x=0.09x = 0.09

According to our STM data taken for x=0.09x = 0.09, the characteristic length scale of gap variation can be determined as LΔ≈58L_{\Delta} \approx58 nm from the autocorrelation coefficients of the gap map (Supplementary Figure 7-Supplementary Figure 7). Compared with ξab≈41.1\xi_{ab} \approx41.1 nm extracted from DOS distribution around a vortex core (Supplementary Figure 7-Supplementary Figure 7), we have LΔ∼(1.5L_{\Delta} \sim(1.5-2)ξab2)\xi_{ab}; this is perfectly consistent with the expectation for a superconducting state with spatially inhomogeneous superconducting order parameter. Previous studies of the local order parameter in strongly disordered superconducting films have congruently revealed self-organized superconducting islands/regions with a size of a few times the coherence length [20, 21, 22, 23]. Our observations in CsV3_3Sb4.91_{4.91}Sn0.09_{0.09} strongly imply that the superconducting gap Δ\Delta varies over a spatial distance set by (but not necessarily precisely equal to) ξab\xi_{ab}. The close correspondence between these two length scales LΔL_{\Delta} and ξab\xi_{ab} verifies that the variation of Δ\Delta (over a distance of a few tens of nanometers) is not an arbitrary long-wavelength artifact, but rather reflects self-organized formation of inhomogeneous superconductivity induced by pair-breaking scattering stemming from short-ranged disorder potential (see further descriptions in Supplementary Note 15).

We further point out that the most likely origin of this pair-breaking disorder potential is the short-ranged charge stripes in Sn-doped CsV3Sb5\mathrm{CsV}_{3}\mathrm{Sb}_{5}, as emphasized in the discussion of the manuscript. According to data from other groups, the correlation length of the short-ranged charge-stripe order is 6–18 nm in CsV3Sb5−xSnx\mathrm{CsV}_{3}\mathrm{Sb}_{5-x}\mathrm{Sn}_{x} with x=0.15x = 0.15 [24]. In our samples, the correlation length of the short-ranged charge-stripe can be longer than this (and becomes close to ξab\xi_{ab}), considering that the CDW correlation length appears to decrease with increasing xx [25]. It has been proposed in several influential theoretical works on cuprate superconductors [26, 27, 28] that when the Cooper pair coherence length is comparable to the correlation length of the disorder potential, the relevant pair-breaking causes the pair-field amplitude to be spatially heterogeneous. Consequently, the short-ranged charge stripe order with a correlation length of a few tens of nanometers promisingly serves as the source of pair-breaking scattering in our samples, given that the superconducting order parameter changes its sign in momentum space.

Supplementary Note 8

Spatially inhomogeneous pair breaking revealed by local tunneling spectra in x=0.09x = 0.09 sample

To verify the spatially inhomogeneous superconductivity in CsV3Sb4.91Sn0.09\mathrm{CsV}_{3}\mathrm{Sb}_{4.91}\mathrm{Sn}_{0.09}, we performed spectroscopic-imaging STM measurements in a 40 nm ×\times 40 nm field of view. The topographic image and the corresponding Sn dopant distribution are shown in Supplementary Fig. 8a and b. Similar to the data in main text Fig. 3, Sn dopants are distributed rather uniformly without evident clustering. In contrast, the superconducting gap map Δ(r)\Delta(r) exhibits a pronounced spatial variation over a length scale of several tens of nanometers (Supplementary Fig. 8c). The histogram of Δ(r)\Delta(r) gives an average gap value Δ‾=303 μeV\overline{\Delta} = 303\ \mu\mathrm{eV} with a standard deviation σ=16.4 μeV\sigma= 16.4\ \mu\mathrm{eV}, corresponding to σ/Δ‾=0.054\sigma/\overline{\Delta} = 0.054 (Supplementary Fig. 8e). This value is close to that obtained in main text Fig. 3, confirming that the superconducting gap inhomogeneity is reproducible in different regions of the same composition.

Moreover, similar to the field of view in main text Fig. 3, local spectra with a larger gap exhibit sharper coherence peaks and a deeper zero-bias suppression, implying a positive correlation between Δ(r)\Delta(r) and H(r)H(r) in this independent region (Supplementary Fig. 8d, f and g). This correlation suggests that the spatial variation of Δ\Delta is accompanied by gap filling and coherence-peak smearing, as expected for an inhomogeneous pair-breaking effect.

To examine whether the spectral evolution can be attributed to spatially varying pair breaking, we fitted the local tunneling spectra using the Dynes formula, N(E)=Re⁡[(E−iΓ)/(E−iΓ)2−Δ(θ)2]N(E) = \operatorname{Re}[(E - i\Gamma)/\sqrt{(E - i\Gamma)^2 - \Delta(\theta)^2}], where Γ\Gamma denotes the pair-breaking parameter. The superconducting gap was taken as a nodeless form with sixfold in-plane anisotropy, Δ(θ)=Δ0+Δ6cos⁡(6θ)\Delta(\theta) = \Delta_0 + \Delta_6\cos(6\theta). A representative fit is shown in Supplementary Fig. 8h. By applying the same fitting procedure pixel by pixel to the dII/dVV map, we obtained the spatial distribution of Γ(r)\Gamma(r), as displayed in Supplementary Fig. 8i.

We then compared Γ(r)\Gamma(r) with the superconducting gap map Δ(r)\Delta(r). Γ(r)\Gamma(r) is spatially inhomogeneous and anti-correlated with Δ(r)\Delta(r): regions with smaller superconducting gaps exhibit larger Γ\Gamma, whereas larger-gap regions show weaker pair breaking. This trend is summarized by the Δ\Delta-Γ\Gamma density plot in Supplementary Fig. 8j and is further confirmed by the negative cross-correlation between Δ(r)\Delta(r) and Γ(r)\Gamma(r) in Supplementary Fig. 8k. These results indicate that the gap filling and suppression of coherence peaks cannot be described by a simple reduction of the gap with spatially constant broadening, but instead point to spatially inhomogeneous pair breaking as a likely origin of the observed superconducting gap inhomogeneity.

Spatially inhomogeneous pair breaking in CsV3Sb4.91Sn0.09

Figure Supplementary 8. Spatially inhomogeneous pair breaking in CsV3Sb4.91Sn0.09\mathrm{CsV_3Sb_{4.91}Sn_{0.09}}. a–d, Topographic image (a), dopant distribution (b), gap map (c) and gap-depth map (d) of a 40 nm ×\times 40 nm field of view. e, Histogram showing the distribution of the gap amplitude in c. f, dI/dV\mathrm{d}I/\mathrm{d}V linecut along the arrow in c, showing the spatial variation in the superconducting gap. The dashed white line serves as a reference. g, Gap depth (HH) versus gap size (Δ\Delta) along the linecut, revealing a positive correlation. h, Representative local tunneling spectrum and fit using a nodeless superconducting gap with sixfold rotational symmetry. i, Spatial distribution of the fitted pair-breaking parameter Γ(r)\Gamma(r) in the same region of c. j, Density plot of Γ\Gamma versus Δ\Delta, showing a clear anti-correlation between the fitted pair-breaking parameter and the local superconducting gap. k, Azimuthally averaged cross-correlation coefficients between the gap amplitude (c) versus the gap depth (d, red curve), the impurity dopants (b, green curve) and the pair-breaking parameter (i, blue curve).

Absence of inhomogeneous strain effects in the x=0.09x = 0.09 sample

It is well-established that the residual strain fields in a superconductor can effectively influence its superconducting properties [29]. If an inhomogeneous strain effect exists, it is likely to equally affect samples with all doping levels xx from 0 to 0.30; there must be specific reasons why the heterogeneous superconducting state only emerges within a narrow window of xx (most profoundly, x=0.07x = 0.07 and 0.09), where the single-QQ stripelike CDW is also the most pronounced [25]. To nail down the influence of internal strain, we have conducted a series of experiments. These new data not only confirm our conclusions but also provide deeper insights into the unusual properties of stripe-ordered kagome lattices.

(i). We had measured the magnetoresistance (MR) and magnetic torque τ(H)\tau(H) in two more CsV3_3Sb5−x_{5-x}Snx_x samples with x=0.09x = 0.09 and the results are shown in Supplementary Figure 9. Similar to the behavior displayed in main text Fig. 2e and f, the diamagnetic hysteresis loop in τ(H)\tau(H) of these two samples closes at a magnetic field HirrH_{\mathrm{irr}} where the resistivity nearly recovers its normal-state value; HirrH_{\mathrm{irr}} appears to be much higher than the vortex depinning field determined from the termination of the zero resistivity, which is quite rare in type-II superconductors. The consistency among observations in all x=0.09x = 0.09 samples indicates that a coexistence of magnetic irreversibility and strongly dissipative transport is an inherent property of this composition (and is not caused by extrinsic mechanisms), verifying our identification of the heterogeneous superconducting state therein.

Magnetoresistance and magnetic torque measurements in two additional x = 0.09 samples

Supplementary Figure 9. The magnetoresistance (MR) and magnetic torque τ(H)\tau(H) measured in two additional x=0.09x = 0.09 samples (#1 and #2). A comparison of the torque magnetometry data (a, c) and ρxx(H)\rho_{xx}(H) (b, d) measured in CsV3_3Sb4.91_{4.91}Sn0.09_{0.09} samples #1 (a and b) and #2 (c and d) under in-plane HH at T=0.5T = 0.5 K (olive), 1.5 K (orange) and 2.5 K (red). Dashed vertical lines denote the position of the onsets of the dissipative state (presumably the depinning field).

(ii). Temperature cycling has been used as an effective method to modify residual strains across the sample [29]. We have measured the in-plane resistivity ρxx\rho_{\mathrm{xx}} during repeated temperature cycling as plotted in Supplementary Figure 10. In practice, an x=0.09x = 0.09 sample was subjected to five successive thermal cycles within a temperature range of 1.8 to 5 K (as illustrated in Supplementary Figure 10); ρxx(T)\rho_{\mathrm{xx}}(T) was collected during the cooling process of each cycle. We adopted a slow cooling rate of 3.3 mK/s (0.2 K/min) to effectively modify the strain inhomogeneity within the sample. As shown in Supplementary Figure 10 and Supplementary Figure 10, the ρxx(T)\rho_{\mathrm{xx}}(T) data taken during the five cycles --- including the broadened superconducting transition --- fall exactly on top of each other, exhibiting no visible dependence on the history of temperature change. We thus infer that the influence of strain inhomogeneity on the transport behavior of CsV3_3Sb4.91_{4.91}Sn0.09_{0.09} is negligible.

Resistivity measurement during repeated thermal cycles across the superconducting transition

Supplementary Figure 10. Resistivity measurement during repeated thermal cycles across the superconducting transition. a, A sketch showing a total of five thermal cycles over the temperature range from 1.8 to 5 K; ρxx(T)\rho_{\mathrm{xx}}(T) was measured during the cooling process of each cycle. b, ρxx(T)\rho_{\mathrm{xx}}(T) curves obtained for each cycle, which are shifted vertically for clarity. c, ρxx(T)\rho_{\mathrm{xx}}(T) data without vertical offsets.

(iii). To further examine whether the observed superconducting inhomogeneity could originate from local strain, we analyzed the strain fields in two surface regions on an x=0.09x = 0.09 sample; within each region, pronounced spatial inhomogeneity of the superconducting gap can be observed. The topographies and corresponding superconducting gap maps for the two fields of view (with sizes of 40 × 40 and 60 × 60 nm2^2, respectively) are displayed in Supplementary Figure 11, Supplementary Figure 11 and Supplementary Figure 11, Supplementary Figure 11, respectively. For each region, we extracted the strain components along the three Bragg directions, UaaU_{\mathrm{aa}}, UbbU_{\mathrm{bb}}, and UccU_{\mathrm{cc}}, as shown in Supplementary Figure 11-Supplementary Figure 11 and Supplementary Figure 11-Supplementary Figure 11, respectively.

Strain analysis based on STM measurements on a sample with x = 0.09

Supplementary Figure 11. Strain analysis based on STM measurements on a sample with x=0.09x = 0.09. a, b, Topographic image T(r)T(\mathbf{r}) (a) and superconducting gap map Δ(r)\Delta(\mathbf{r}) (b) in the first field of view with an area of 40×4040 \times40 nm2^2. c, The cross-correlation coefficients between Δ(r)\Delta(\mathbf{r}) and the strain components UaaU_{aa} (red), UbbU_{bb} (olive), and UccU_{cc} (orange) along three Bragg directions. d-f, Strain maps extracted along the three Bragg directions, UaaU_{aa} (d), UbbU_{bb} (e), and UccU_{cc} (f). g-l, Same as a-f but for data taken within a second field of view with an area of 60×6060 \times60 nm2^2. In both fields of view, the strain distributions do not show a global pattern matching the superconducting gap inhomogeneity; the correlation coefficients between the strain distribution and gap distribution are close to zero for all directions.

The most important implication of this study is the absence of correlation between the spatial distribution of the superconducting gap, Δ(r)\Delta(\mathbf{r}), and any of the extracted strain components. None of the strain maps show a global spatial pattern that matches the inhomogeneity of Δ(r)\Delta(\mathbf{r}) [see the distinct trends of spatial variation when contrasting the patterns in Supplementary Figure 11-Supplementary Figure 11(Supplementary Figure 11-Supplementary Figure 11) with Supplementary Figure 11(Supplementary Figure 11)]. This is further confirmed by the cross-correlation analysis between the strain fields and the gap maps. As shown in Supplementary Figure 11 and Supplementary Figure 11, the correlation coefficients remain close to zero for all three strain components. Therefore, the superconducting gap inhomogeneity observed in the x=0.09x = 0.09 sample cannot be attributed to a local strain distribution since the latter fails to track the local superconducting gap.

Combining (i), (ii) and (iii), we can confidently conclude that the unique properties of CsV3_3Sb4.91_{4.91}Sn0.09_{0.09}, in particular the heterogeneous nature of its superconducting state highlighted by a spatial distribution of the superconducting gap, are more likely intrinsic for this compound. We cannot find evidence in our transport, torque magnetometry and STM studies that randomly distributed strain fields across the sample contributed to our observations, to any extent.

Influence of surface Cs clusters on the local superconducting gap

Another trivial origin of the STM-resolved spatial distribution of the superconducting gap is the variation of the chemical environment at the surface. The local superconducting gap could change at boundaries between Cs-diluted and Cs-rich regions in Ta-doped CsV3Sb5\mathrm{CsV}_{3}\mathrm{Sb}_{5} samples, probably due to surface electronic doping effects [30]. Therefore, one may doubt that the observed gap variation can originate from the Cs clusters in the surrounding area. In the following we present two key facts that exclude surface Cs clusters as a possible reason for the inhomogeneity in our case.

First, a large field of view that includes the area shown in Supplementary Fig. 8 is displayed in Supplementary Figure 12. The gradual variation in the superconducting gap from the up-left to the bottom-right (Supplementary Fig. 8c), at first glance, does not show any relationship with the surrounding Cs clusters. Second, we also found boundaries between Cs-diluted and Cs-rich regions in our Sn-doped samples, and, similar to the case reported in Ref. [30], the gap variation occurred abruptly at the boundary (Supplementary Figure 12-Supplementary Figure 12). This abrupt change is in sharp contrast to the intrinsic gap inhomogeneity that is more continuous over the length scale of ξab\xi_{ab} as discussed in the main text. Moreover, near such a Cs boundary, a spectrum with a larger superconducting gap exhibits lower coherence peaks (Supplementary Figure 12), which is also different from the data shown in main text Fig. 3. We note that for the data shown in Supplementary Figure 12-Supplementary Figure 12, a superconducting Nb tip was used with Δtip≈1.3\Delta_{\mathrm{tip}} \approx1.3 meV.

Influence of the surface Cs cluster on the local superconducting gap

Supplementary Figure 12. Influence of the surface Cs cluster on the local superconducting gap. a, STM topographic image in a large FOV which includes the region shown in Supplementary Fig. 8. b, Topographic image depicting a boundary between Cs-diluted and Cs-rich regions on the Sb surface. c, dII/dVV linecut along the orange line crossing the boundary in panel b. d, Superconducting gap variation along the line. e, Representative spectra from the Cs-diluted (orange) and Cs-rich (green) regions; a superconducting Nb tip is used with Δtip≈1.3\Delta_{\mathrm{tip}} \approx1.3 meV.

Doping dependence of superconducting gap inhomogeneity

To further exclude the possibility that the superconducting gap inhomogeneity is simply caused by Sn substitution, we compared the spectroscopic properties of CsV3Sb5−xSnx\mathrm{CsV}_{3}\mathrm{Sb}_{5-x}\mathrm{Sn}_{x} samples with x=0.06x = 0.06 (long-range triple-QQ CDW), x=0.09x = 0.09 (short-range single-QQ CDW), x=0.12x = 0.12 (single-QQ CDW with further reduced correlation length) and x=0.30x = 0.30 (likely fluctuating single-QQ CDW or very short-ranged stripelike charge correlation, nearly undistorted kagome lattice) [2, 25]. The zero-bias conductance maps measured in the normal state show that the x=0.30x = 0.30 sample has a much stronger spatial variation of the normal-state density of states than the x=0.09x = 0.09 sample (Supplementary Figure S13 and Figure S13). This is also reflected by the larger normalized standard deviation σ/μ\sigma/\mu of the differential conductance over a wide energy range in x=0.30x = 0.30 (Supplementary Figure S13), indicating that the normal-state electronic environment is more inhomogeneous at higher Sn concentration.

Differential conductance maps, superconducting gap map, gap histogram, linecut, vortex map and spectra for CsV3Sb4.7Sn0.3

Figure S13. Spatial characteristics of the normal and superconducting states in CsV3Sb4.7Sn0.3\mathrm{CsV}_{3}\mathrm{Sb}_{4.7}\mathrm{Sn}_{0.3}. a, b, Differential conductance maps at 0 mV for x=0.09x = 0.09 (a) and x=0.3x = 0.3 (b) measured at 4.2 K. The data were collected in 50 nm ×\times 50 nm FOVs at 4.2 K for x=0.09x = 0.09 and x=0.3x = 0.3. The latter clearly exhibits a more inhomogeneous normal-state DOS. c, Standard deviation (σ\sigma) divided by the mean value (μ\mu) of the differential conductance values at different energies for x=0.09x = 0.09 and x=0.3x = 0.3. d, e, Topography and superconducting gap map in a 50 nm ×\times 50 nm FOV for x=0.3x = 0.3. f, Histogram of the gap amplitude of e. g, dI/dVdI/dV linecut along the purple arrow in e. h, Zero-bias dI/dVdI/dV conductance map with an out-of-plane magnetic field of 0.5 T, showing a superconducting vortex. i, Spectra showing the bound state inside the superconducting vortex in h (green curve), together with that far away from the vortex (orange curve). The presence of Caroli–de Gennes–Matricon vortex states in the x=0.3x = 0.3 sample suggests weaker scattering for this composition compared with x=0.09x = 0.09.

This notwithstanding, the superconducting gap in x=0.30x = 0.30 is rather homogeneous. Supplementary Figure S13 and Figure S13 show the topographic image and superconducting gap map measured in a 50 nm ×\times 50 nm field of view. Despite the strong normal-state inhomogeneity, the distribution of Δ(r)\Delta(r) is narrow, with an average gap value Δˉ=670\bar{\Delta} = 670 μ\mueV, a standard deviation σ=13.7\sigma= 13.7 μ\mueV and σ/Δˉ=0.020\sigma/\bar{\Delta} = 0.020 (Supplementary Figure S13), markedly smaller than σ/Δˉ=0.051\sigma/\bar{\Delta} = 0.051 observed in the stripe-ordered x=0.09x = 0.09 sample. The linecut spectra exhibit nearly unchanged coherence-peak positions across the field of view, further confirming the weak spatial variation of Δ\Delta in x=0.30x = 0.30 (Supplementary Figure S13). The observation of Caroli-de Gennes-Matricon bound states inside the vortex core (Supplementary Figure S13 and Figure S13) further indicates weaker quasiparticle scattering in x=0.30x = 0.30, consistent with its more homogeneous superconducting gap.

More information about the close correlation between the charge-stripe order and spatially inhomogeneous superconductivity has been revealed by STM measurements on two additional compositions, x=0.06x = 0.06 and 0.120.12, on both sides of x=0.09x = 0.09. The x=0.06x = 0.06 sample is positioned in the triple-QQ (2×22 \times2) CDW phase region (see the phase diagram in main text Figure 1b), whereas the x=0.12x = 0.12 sample shows the absence of CDW-related anomaly in charge transport (Supplementary Fig. 3b). Here we elucidate that the superconducting state is nearly homogeneous in both cases.

For x=0.06x = 0.06, the gap map and linecut spectra show only weak spatial variation (Supplementary Figure 14-Supplementary Figure 14). The gap histogram gives an average value Δˉ=425\bar{\Delta} = 425 μ\mueV, a standard deviation σ=5\sigma= 5 μ\mueV, and σ/Δˉ=0.012\sigma/\bar{\Delta} = 0.012 (Supplementary Figure 14), much smaller than σ/Δˉ=0.051\sigma/\bar{\Delta} = 0.051 for the stripe-ordered x=0.09x = 0.09 sample. Similarly, for x=0.12x = 0.12, the gap map and linecut spectra also reveal marginal gap variation (Supplementary Figure 14-Supplementary Figure 14), with Δˉ=390\bar{\Delta} = 390 μ\mueV, σ=4\sigma= 4 μ\mueV, and σ/Δˉ=0.010\sigma/\bar{\Delta} = 0.010, Supplementary Figure 14). The representative spectra in both compositions show fully opened superconducting gaps with negligible residual density of states.

Spatially homogeneous superconducting states in CsV$_3$Sb$_{5-x}$Sn$_x$ samples with $x=0.06$ and $0.12$

Supplementary Figure 14. Spatially homogeneous superconducting states in CsV3_3Sb5−x_{5-x}Snx_x samples with x=0.06x = 0.06 and 0.120.12. a, Topographic image measured on the x=0.06x = 0.06 sample. b, Superconducting gap map Δ(r)\Delta(r) in the same field of view as in a. c, Histogram of the gap values extracted from b. The distribution is narrow, with Δˉ=425\bar{\Delta} = 425 μ\mueV, σ=5\sigma= 5 μ\mueV and σ/Δˉ=0.012\sigma/\bar{\Delta} = 0.012. Inset: representative superconducting spectrum showing a full gap with negligible residual density of states. d, dII/dVV linecut showing a nearly position-independent superconducting gap in x=0.06x = 0.06. e-h, Same analysis as in a-d, but measured on the x=0.12x = 0.12 sample. The gap map and linecut spectra reveal marginal spatial variation of the superconducting gap. The gap histogram gives Δˉ=390\bar{\Delta} = 390 μ\mueV, σ=4\sigma= 4 μ\mueV and σ/Δˉ=0.010\sigma/\bar{\Delta} = 0.010. The narrow gap distributions in both compositions indicate spatially homogeneous superconducting states outside the stripe-ordered x=0.09x = 0.09 regime.

The gap statistics for different doping levels are summarized in Supplementary Table 2. The normalized gap variation σ/Δˉ\sigma/\bar{\Delta} is small for x=0.06x = 0.06, 0.120.12 and 0.300.30, with values of 0.012, 0.010 and 0.020, respectively. By contrast, σ/Δˉ\sigma/\bar{\Delta} reaches a more remarkable value of 0.051 at x=0.09x = 0.09. Therefore, the pronounced superconducting gap inhomogeneity appears uniquely in this compound wherein the charge-stripe-induced band reconstruction can be clearly resolved in QPI (Supplementary Note 12 and Supplementary Figure 15). This strongly suggests that the heterogeneous superconducting state is not a direct consequence of chemical disorder introduced by Sn substitution, but is instead linked to the charge-stripe order (or more precisely, its effectiveness in inducing band reconstruction).

Sn doping level xx0.060.090.120.30
Δˉ\bar{\Delta} (meV)0.4250.3230.3900.670
σ\sigma (meV)0.005(0)0.016(6)0.004(0)0.013(7)
σ/Δˉ\sigma/\bar{\Delta}0.0120.0510.0100.020

Table 2. The mean value Δˉ\bar{\Delta} of the spatially varying superconducting gap Δ(r)\Delta(r), its standard deviation σ\sigma, and the ratio between them, σ/Δˉ\sigma/\bar{\Delta}, determined from STM measurements in CsV3_3Sb5−x_{5-x}Snx_x with x=0.06x = 0.06, 0.090.09, 0.120.12 and 0.300.30.

Spatial correlation between stripe-induced folded-band QPI and superconducting gap in the x=0.09x = 0.09 sample

In our STM measurements, the stripe-related signature is mainly identified from the QPI patterns, where the charge-stripe order folds the quasi-one-dimensional kagome bands and gives rise to additional scattering vectors q′q^\prime and q′′q^{\prime\prime} (Supplementary Figure 15-Supplementary Figure 15). Short-range real-space modulations with a periodicity of approximately 3a03a_0 can also be observed in strained samples (Supplementary Figure 15). However, applying strain may introduce additional complexity, since superconductivity itself can also be tuned by external strain. Therefore, in the following we use the folded-band QPI features as practical fingerprints of stripe-related electronic reconstruction.

In Supplementary Figure 15-Supplementary Figure 15 we compare the normal-state QPI patterns for four representative compositions, x=0.06x = 0.06, 0.090.09, 0.120.12 and 0.300.30. The stripe-induced q′q^\prime and q′′q^{\prime\prime} features are clearly resolved only in the x=0.09x = 0.09 sample, whereas they are absent in the other three compositions. Note that transport measurements also show the absence of CDW-related anomaly in x=0.12x = 0.12 and 0.300.30 (Supplementary Note 2). This indicates a profound electronic band reconstruction induced by the short-range stripelike CDW occurring only for x=0.09x = 0.09 among these four compositions; its disappearance at x=0.12x = 0.12 is likely attributed to the reduced correlation length of the charge-stripe order at higher xx. (In the phase diagram displayed in main text Figure 1b, we thus anticipate that pronounced impact of the single-QQ CDW happens only within a narrow window above x=0.07x = 0.07, as highlighted by the background colour.)

To investigate the relationship between the charge stripe order and the local superconducting gap Δ(r)\Delta(r), we compared the stripe-induced QPI intensity with Δ(r)\Delta(r) in the x=0.09x = 0.09 sample. we performed spatial-resolved Fourier-transformed (FT) analysis on two independent datasets for x=0.09x = 0.09. For each dataset, both QPI and gap map Δ(r)\Delta(r) were measured in the same field of view. Then, for each dataset, we selected two equal-area regions (with nearly identical local Sn concentration) exhibiting distinct local gap amplitudes, labeled as A1 and A2 for dataset #1 (Supplementary fig:16a, b), and B1 and B2 for dataset #2 (Supplementary fig:16g, h), respectively. Here A1 and B1 (A2 and B2) correspond to the relatively larger-gap (smaller-gap) regions. The spatial-resolved FT-QPI maps for all these four regions were obtained and shown in Supplementary fig:16c, d and i, j. This allows us to check whether the characteristic QPI signals for the charge stripe order (q′q' and q′′q'') are stronger in regions with larger superconducting gap.

From Supplementary Figure 16, Supplementary Figure 16 and Supplementary Figure 16, Supplementary Figure 16, a visual inspection finds that the characteristic QPI features of q′q' and q′′q'' appear to be more pronounced in the larger-gap region A1 (B1) as compared to A2 (B2). This can be cross-checked by quantitatively comparing their FT intensity. We first look into the signal at q′′q'': the linecuts across q′′q'' are shown in Supplementary Figure 16 and Supplementary Figure 16 (taken along the arrows in Supplementary Figure 16, Supplementary Figure 16 and Supplementary Figure 16, Supplementary Figure 16), and one can clearly see that its intensity is larger in A1 (B1) compared with that in A2 (B2). In these linecuts, q′q' is overlapped with the strong QPI signal of Sb p-orbital (the circular shape QPI), which obscures a direct comparison of the q′q' intensities. Instead, we can plot the averaged intensity of q′q' within a qq-space window away from the Sb-p-orbital QPI patterns as marked by the orange rectangles in Supplementary Figure 16, Supplementary Figure 16, Supplementary Figure 16 and Supplementary Figure 16. The results are shown in Supplementary Figure 16 and Supplementary Figure 16, and the intensity of q′q' is also larger in the regions with larger superconducting gap. The consistent results of q′q' and q′′q'' demonstrate that the regions with stronger stripe-induced band folding also exhibit larger superconducting gap. We note that in these regions the number of local Sn dopants (the number of scattering centers) is nearly identical (205 and 207), thus it is unlikely to be the reason for the observed different QPI intensity. This suggests a positive correlation between the local strength of charge stripe and the local amplitude of the superconducting order parameter, instead of a competition.

Spatial correlation between stripe-induced folded-band QPI and superconducting gap for CsV3Sb4.91Sn0.09

Supplementary Figure 16. Spatial correlation between stripe-induced folded-band QPI and superconducting gap for CsV3_3Sb4.91_{4.91}Sn0.09_{0.09}. a, b, Superconducting gap map Δ(r)\Delta(r) (a) and differential-conductance map g(r)g(r) (b) measured in the first field of view. Two equal-area regions with relatively large and small Δ\Delta are marked as A1 and A2, respectively. c, d, FT-QPI maps obtained from A1 (c) and A2 (d). The stripe-induced folded-band QPI features q′q' and q′′q'' are highlighted by orange and green colors in c, respectively. e, Linecuts through q′′q'' along the direction marked by the black arrows in c and d. The green shaded region marks the q′′q'' feature. f, Averaged FT-QPI intensity within the momentum-space window (orange shaded regions in c and d) around q′q' for A1 and A2. g–l, Same analysis as in a–f, but for another field of view wherein the equal-area regions with relatively large and small Δ\Delta are marked as B1 and B2, respectively. In both fields of view, the larger-gap region A1(B1) shows higher intensity of stripe-induced folded-band QPI than A2(B2).

Hence, according to the FT-QPI signatures, our data mark a clear departure from the simple anti-correlation between the charge stripe order and the local superconducting gap; in contrast, our observations imply that these two quantities increase in tandem. This argues against the crude picture of spatial-dependent competition between the two orders (in which a stronger stripe-related reconstruction directly suppresses the superconductivity). Alternatively, results shown in Supplementary Figure 16 suggest that the observed heterogeneous superconducting state is the ramification of unusual corporation of the charge stripe and superconducting pairing instabilities.

Combined with the analysis of the local pair-breaking parameter Γ\Gamma presented in Supplementary Note 8, this positive correlation can be understood phenomenologically. The larger-gap regions exhibit enhanced stripe-induced folded-band QPI signals but weaker pair breaking, as reflected by the smaller Γ\Gamma. We propose that stronger q′/q′′q'/q'' QPI intensity may reflect stripe correlations that are locally more coherent in phase, which generate a more well-defined band-folding signal while producing weaker pair-breaking scattering. By contrast, regions with more disrupted or frustrated stripe correlations may give weaker folded-band QPI signals but stronger pair breaking, leading to an enhanced Γ\Gamma and a reduced local gap Δ\Delta. We emphasize that this is a phenomenological interpretation; a microscopic understanding of how short-range charge stripes modulate superconducting pairing and pair breaking requires further theoretical work.

Supplementary Note 13:

Analysis of the specific heat

The electronic specific heat CeC_{\mathrm{e}} of CsV3_3Sb5_5-xSnx_x (x=0,0.06,0.07,0.09,0.12x = 0, 0.06, 0.07, 0.09, 0.12 and 0.30.3) was obtained by subtracting CphC_{\mathrm{ph}} and CshC_{\mathrm{sh}} from the raw data (see Methods), as plotted in Supplementary Figure 17. We analyzed the Ce(T)/TC_{\mathrm{e}}(T)/T data in the superconducting state using the BCS α\alpha-model [31, 32] and the results are presented in Supplementary Figure 18.

Analysis of electronic specific heat of CsV3Sb5-xSnx

Supplementary Figure 18. Supplementary Fig. 18. Analysis of electronic specific heat CeC_{\rm e} of CsV3_3Sb5−x_{5-x}Snx_x. a-f, Fitting the Ce/TC_{\rm e}/T data to the BCS α\alpha-model (solid lines) for x=0x = 0 (a), x=0.06x = 0.06 (b), x=0.07x = 0.07 (c), x=0.09x = 0.09 (d), x=0.12x = 0.12 (e) and x=0.3x = 0.3 (f). Red and blue full lines represent the single-gap and two-gap α\alpha-models, respectively (all assuming full gaps and a residual term γ0\gamma_0). g, The entropy difference ΔS=SS−SN\Delta S = S_{\rm S} - S_{\rm N} between the electronic entropy of the superconducting state (SSS_{\rm S}) and the normal state (SNS_{\rm N}) for x=0.07x = 0.07 (orange) and x=0.09x = 0.09 (olive). The solid lines (dashed lines) represent the results of integrating Ce/TC_{\rm e}/T with the assumption of saturation towards γ0\gamma_0 (decrease towards zero) at T<0.2T < 0.2 K, as denoted by the red solid curves (gray dashed curves) in c and d. Only the former assumption satisfies the entropy balance condition that ΔS\Delta S becomes zero at T≈TcST \approx T_{\rm c}^{\rm S}. h, The specific heat jump ΔC/γnTc\Delta C/\gamma_{\rm n}T_{\rm c} (γn\gamma_{\rm n} is the Sommerfeld coefficient in the normal state, TcT_{\rm c} is determined from the maximum of Ce/TC_{\rm e}/T) plotted against the Sn doping level xx. Note that the residual term γ0\gamma_0 is not subtracted from γn\gamma_{\rm n}. i, Tests of the exponential TT dependence of Ce/γnTcC_{\rm e}/\gamma_{\rm n}T_{\rm c} [47]. Black dashed line indicates the expected behavior in a BCS single-gap weak-coupling limit.

For pristine CsV3Sb5\mathrm{CsV}_{3}\mathrm{Sb}_{5}, the data are incompatible with a single-gap α\alpha-model, but can be successfully described by a two-band model with superconducting gaps ΔL=0.4\Delta_{\mathrm{L}} = 0.4 meV, ΔS=0.14\Delta_{\mathrm{S}} = 0.14 meV and a residual γ0=4.5\gamma_{0} = 4.5 mJ mol−1^{-1} K−1^{-1} (Supplementary Figure 18). This result adds to the existing evidence for nodeless multigap superconductivity in CsV3Sb5\mathrm{CsV}_{3}\mathrm{Sb}_{5} [33, 34, 35, 36, 37]. Moreover, the substantially reduced specific heat jump ΔCe/γnTc≈0.72\Delta C_{\mathrm{e}}/\gamma_{\mathrm{n}}T_{\mathrm{c}} \approx0.72 (here TcT_{\mathrm{c}} was taken as the temperature where Ce/TC_{\mathrm{e}}/T reaches its maximum) compared with the BCS value 1.43 (Supplementary Figure 18) can be associated with both the superconducting gap anisotropy [38] and the existence of multiple gaps [39, 40]. The data measured in the x=0.06x = 0.06 sample (which also possesses long-range triple-QQ CDW) appear to show qualitatively consistent two-gap behavior with the pristine sample (Supplementary Figure 18).

For the sample with x=0.07x = 0.07, Ce(T)C_{\mathrm{e}}(T) (T<0.8T < 0.8 K) can be fitted by the α\alpha-model with one full gap (Δ=0.17\Delta= 0.17 meV) with a large residual linear term γ0≈17\gamma_0 \approx17 mJ mol−1^{-1} K−1^{-1} (Supplementary Figure 18). Similarly, Ce(T)C_{\mathrm{e}}(T) (T<1T < 1 K) for x=0.09x = 0.09 can be fitted by the single-gap α\alpha-model assuming Δ=0.27\Delta= 0.27 meV with γ0≈11.7\gamma_0 \approx11.7 mJ mol−1^{-1} K−1^{-1} (Supplementary Figure 18). At T→TcT \to T_{\mathrm{c}}, Ce(T)C_{\mathrm{e}}(T) deviates from this fit, with the specific heat jump profoundly suppressed from the model’s prediction (main text Fig. 4a and Supplementary Figure 18, Supplementary Figure 18). This phenomenon further corroborates a distribution of local TcT_{\mathrm{c}} that smears the sharp jump of CeC_{\mathrm{e}} at T=TcT = T_{\mathrm{c}}, yielding a broad and stunted specific heat anomaly (whose height is further reduced by the large proportion of normal fluid, Supplementary Figure 18). As such, the gap value provided by the fit below 1 K should be taken as a spatial average over the sample.

In particular, we stress that the ostensible saturation of Ce/TC_{\mathrm{e}}/T at a notable non-zero value (≈γ0\approx\gamma_0) at the lowest TT for x=0.07x = 0.07 and 0.09 sample can only be understood by proposing large residual unpaired DOS; the direct observation of these unpaired quasiparticles in STM data (main text Fig. 4e-h) serves as the most compelling support. Such phenomenon cannot be explained by the presence of a very small second superconducting gap ΔS\Delta_{\mathrm{S}}. As displayed in Supplementary Figure 18 and Supplementary Figure 18, a two-gap α\alpha-model assuming an extremely small ΔS\Delta_{\mathrm{S}} (blue solid lines) fails to reproduce the measured profile of Ce/TC_{\mathrm{e}}/T in both x=0.07x = 0.07 and x=0.09x = 0.09, mostly manifested by the absence of the humplike anomaly heralding the low-TT drop of Ce/TC_{\mathrm{e}}/T caused by ΔS\Delta_{\mathrm{S}}. The occurrence of this anomaly has been ubiquitously observed in superconductors with small gaps, e.g., Nb3_3Sn [41], Lu2_2Fe3_3Si5_5 [39], KFe2_2As2_2 [40] and FeSe [42]. Moreover, the presence of such a small ΔS\Delta_{\mathrm{S}} yielded by the fits, which is below 0.05 meV (ΔS<0.3kBTc\Delta_{\mathrm{S}} < 0.3 k_{\mathrm{B}}T_{\mathrm{c}} for x=0.09x = 0.09), indisputably evades our STM measurements down to 20 mK (main text Fig. 4c) in the k-space (Supplementary Note 16).

The analysis based on the entropy balance arguments, i.e., the entropy SelS_{\mathrm{el}} of the electronic system must recovers to the value equal to the normal-state entropy at a temperature above the second-order superconducting transition (T≳TcT \gtrsim T_{\mathrm{c}}) [43, 44], provides another strong argument against the presence of a small ΔS\Delta_{\mathrm{S}}. The entropy calculations presented in Supplementary Figure 18 with the assumption of a constant residual DOS γ0\gamma_0 (solid curves) generally fulfill the entropy balance condition. If Ce/TC_{\mathrm{e}}/T abruptly drops to zero at T<0.2T < 0.2 K owing to the full opening of the small gap ΔS\Delta_{\mathrm{S}} (dashed lines in Supplementary Figure 18 and Supplementary Figure 18), the entropy balance will be broken as demonstrated by the dashed curves in Supplementary Figure 18, which challenges the basic understanding of superconductivity.

When the charge-stripe order is almost collapsed at x=0.30x = 0.30, Ce(T)C_{\mathrm{e}}(T) falls close to the single-gap α\alpha-model fit with Δ=0.52\Delta= 0.52 meV and a small residual term γ0=2.4\gamma_0 = 2.4 mJ mol−1^{-1} K−1^{-1} (Supplementary Figure 18), indicating that a more isotropic full superconducting gap is established. Similar suppression of gap anisotropy upon chemical substitution has been observed in other doped CsV3_3Sb5_5 superconductors [30, 45, 46]. The value of Δ\Delta corresponds to 2Δ/kBTc=3.542\Delta/k_{\mathrm{B}}T_{\mathrm{c}} = 3.54 close to the weak-coupling BCS value 3.53 (correspondingly, ΔCe/γnTc≈1.59\Delta C_{\mathrm{e}}/\gamma_{\mathrm{n}}T_{\mathrm{c}} \approx1.59, Supplementary Figure 18); the empirical relation Ce/γnTc∝exp⁡[−1.44(Tc/T)]C_{\mathrm{e}}/\gamma_{\mathrm{n}}T_{\mathrm{c}} \propto\exp[-1.44(T_{\mathrm{c}}/T)] holds for CsV3_3Sb4.70_{4.70}Sn0.30_{0.30} over a range 1.6<Tc/T<2.71.6 < T_{\mathrm{c}}/T < 2.7, also in accord with the prediction of the weak-coupling BCS theory [47]. Thereby, this compound appears to be a standard BCS superconductor. The data for x=0.06x = 0.06 qualitatively matches that for x=0.30x = 0.30 yet with a larger γ0\gamma_0 (Supplementary Figure 18). It should be mentioned that in both the triple-QQ CDW (x=0x = 0, 0.060.06) and fluctuating CDW (x=0.12x = 0.12, 0.300.30) phases, γ0\gamma_0 is constantly smaller than 6 mJ mol−1^{-1} K−1^{-1}; such an amplitude barely surpasses the uncertainties in our specific heat analysis (main text Fig. 4b), hence obscuring the unambiguous determination of intrinsic nature of the residual term.

These results of specific heat analysis strongly imply nodeless superconductivity across the CsV3_3Sb5−x_{5-x}Snx_x series, with the anisotropy and/or orbital-dependent feature of Δ\Delta weakened upon Sn doping. We find no evidence for nodal superconductivity. Remarkably, CeC_{\rm e} of the x=0.09x = 0.09 sample cannot be fitted by the form Ce(T)∝T2C_{\rm e}(T) \propto T^2 describing a gap structure with line nodes (main text Fig. 4a). Even the superconducting state is prone to nonmagnetic pair breaking as implied by the enormous γ0\gamma_0 and is thus supposedly sign changing [48, 49, 50], it is still more likely to be fully gapped rather than nodal (see also Supplementary Note 16 for further evidence). Nonetheless, the nodal pairing states (e.g., ff-wave pairing in a kagome lattice [51, 52]) cannot be completely ruled out because the contribution of nodal quasiparticles might be masked by the abundant low-energy excitations provoked by pair-breaking scattering [50, 53].

Absence of localization effects in CsV3Sb5−xSnx\mathrm{CsV_3Sb_{5-x}Sn_x}

It has been well established that conventional (BCS-type ss-wave) superconductivity exhibits remarkable resilience against Anderson localization and persists even in strongly disordered systems in the absence of magnetic impurities: For spatial dimension dd, appreciable disorder-induced suppression of the superconducting order parameter Δ\Delta (and strong inhomogeneity of Δ\Delta) occurs when [54, 55]:

DΔξlocd<1,(7)\mathcal{D}\Delta\xi_{\mathrm{loc}}^{d} < 1, \tag*{(7)}

here D\mathcal{D} is the average DOS at the Fermi energy EFE_{\mathrm{F}} and ξloc\xi_{\mathrm{loc}} is the localization length. In two dimensions (2D), a perturbative estimate ξloc≈lexp⁡[(π/2)kFl]\xi_{\mathrm{loc}} \approx l\exp[(\pi/2)k_{\mathrm{F}}l] [56] works across the transition from weak to strong disorder (kFk_{\mathrm{F}} is the Fermi wave vector, ll is the mean free path); kFlk_{\mathrm{F}}l is frequently noted as the Ioffe-Regel parameter characterizing the strength of localization (the Anderson critical regime is entered when kFl≲1k_{\mathrm{F}}l \lesssim1 [57]). For disordered superconducting films (d=2d=2), Eq. (7) converts to a threshold for the occurrence of superconductor-insulator (S-I) transition: ξloc≃ξsuper\xi_{\mathrm{loc}} \simeq\xi_{\mathrm{super}}, where ξsuper=(ξBCSl)1/2\xi_{\mathrm{super}}=(\xi_{\mathrm{BCS}}l)^{1/2} is the superconducting coherence length in the dirty limit, ξBCS=ℏvF/(πΔ)\xi_{\mathrm{BCS}}=\hbar v_{\mathrm{F}}/(\pi\Delta) is the BCS coherence length (vF=ℏkF/m∗v_{\mathrm{F}}=\hbar k_{\mathrm{F}}/m^* is the Fermi velocity, m∗m^* is the effective mass); the experimentally determined S-I transition happens at a larger localization scale with ξloc\xi_{\mathrm{loc}} varying from ∼2\sim2 to ∼30 ξsuper\sim30\,\xi_{\mathrm{super}} [58, 59] and a pronounced tendency of spatially nonuniform Δ\Delta develops in the vicinity of this threshold.

Now we demonstrate that our CsV3Sb5−xSnx\mathrm{CsV_3Sb_{5-x}Sn_x} (x=0.07x=0.07, 0.090.09) samples are far from these thresholds for strong impacts of disorder on superconductivity. In general, the Ioffe-Regel parameter kFlk_{\mathrm{F}}l can be estimated from the residual resistivity extrapolated to T=0T=0 [ρ0=(ne2τ/m∗)−1\rho_0=(ne^2\tau/m^*)^{-1} in a simple Drude model, τ\tau is a characteristic relaxation time] (Supplementary Fig. 3a, inset); the carrier density nn can be extracted from the Hall coefficient RH=(ne)−1R_{\mathrm{H}}=(ne)^{-1}. Considering the multiband electronic structure of the Cs135 family [60], we employed a two-band model [61] with electron and hole carriers to fit the Hall resistivity ρxy(H)\rho_{xy}(H) and magnetoresistance ρxx(H)\rho_{xx}(H) of CsV3Sb4.91Sn0.09\mathrm{CsV_3Sb_{4.91}Sn_{0.09}} at T=5T=5 K:

ρxx=1e(nhμh+neμe)+(nhμh+neμe)μhμeB2(nhμh+neμe)2+(nh−ne)2μh2μe2B2,(8)\rho_{xx}=\frac{1}{e}\frac{(n_{\mathrm{h}}\mu_{\mathrm{h}}+n_{\mathrm{e}}\mu_{\mathrm{e}})+(n_{\mathrm{h}}\mu_{\mathrm{h}}+n_{\mathrm{e}}\mu_{\mathrm{e}})\mu_{\mathrm{h}}\mu_{\mathrm{e}}B^2}{(n_{\mathrm{h}}\mu_{\mathrm{h}}+n_{\mathrm{e}}\mu_{\mathrm{e}})^2+(n_{\mathrm{h}}-n_{\mathrm{e}})^2\mu_{\mathrm{h}}^2\mu_{\mathrm{e}}^2B^2}, \tag*{(8)}
ρxy=Be(nhμh2−neμe2)+(nh−ne)μh2μe2B2(nhμh+neμe)2+(nh−ne)2μh2μe2B2.(9)\rho_{xy}=\frac{B}{e}\frac{(n_{\mathrm{h}}\mu_{\mathrm{h}}^2-n_{\mathrm{e}}\mu_{\mathrm{e}}^2)+(n_{\mathrm{h}}-n_{\mathrm{e}})\mu_{\mathrm{h}}^2\mu_{\mathrm{e}}^2B^2}{(n_{\mathrm{h}}\mu_{\mathrm{h}}+n_{\mathrm{e}}\mu_{\mathrm{e}})^2+(n_{\mathrm{h}}-n_{\mathrm{e}})^2\mu_{\mathrm{h}}^2\mu_{\mathrm{e}}^2B^2}. \tag*{(9)}

In Eqs. (8) and (9), the subscripts hh and ee represent hole and electron carriers, respectively, and μ=eτ/m∗\mu=e\tau/m^* is the carrier mobility. Fitting the experimental data to these expressions, as shown in Supplementary Figure 19 and Supplementary Figure 19, we can obtain the following parameters for CsV3Sb4.91Sn0.09\mathrm{CsV_3Sb_{4.91}Sn_{0.09}} (at T=T= 5 K): ne=5.5×1020 cm−3n_e = 5.5 \times10^{20}\ \mathrm{cm}^{-3}, nh=5.9×1020 cm−3n_h = 5.9 \times10^{20}\ \mathrm{cm}^{-3}, μe=72 cm2 V−1 s−1\mu_e = 72\ \mathrm{cm}^{2}\ \mathrm{V}^{-1}\ \mathrm{s}^{-1} and μh=65 cm2 V−1 s−1\mu_h = 65\ \mathrm{cm}^{2}\ \mathrm{V}^{-1}\ \mathrm{s}^{-1}. Starting from quasi-2D cylinder-shaped Fermi surfaces (n=kF2/2πcn = k_F^2/2\pi c) and three-dimensional (3D) spherical Fermi surfaces (n=kF3/3π2n = k_F^3/3\pi^2), the derived results of kFlk_F l and ξloc\xi_{\mathrm{loc}} (only for the 2D case) are listed in Supplementary Table 3. The fact that kFlk_F l is on the order of 10 and hence the gigantic 2D ξloc≫ξsuper\xi_{\mathrm{loc}} \gg\xi_{\mathrm{super}} (ξab≃20\xi_{ab} \simeq20–40 nm, Supplementary Note 3) excludes the presence of strong localization effect in the x=0.09x = 0.09 sample: It is far on the metallic side of the above-mentioned thresholds for appreciable localization effects. Therefore, spatial inhomogeneity of Δ\Delta ought to vanish in the case of BCS ss-wave superconductivity because of the weakness of disorder potential. The same is true for x=0.07x = 0.07, since ρ0\rho_0 of this sample is lower than that of x=0.09x = 0.09, suggesting better metallicity (Supplementary fig:3a; note that the heterogeneous signatures of superconductivity are strongest at x=0.07x = 0.07, see main text).

Hall resistivity and two-band model fits

Supplementary Figure 19. Hall resistivity of CsV3_3Sb4.91_{4.91}Sn0.09_{0.09} and two-band model fits. a, Hall resistivity ρxy\rho_{xy} plotted as a function of HH up to 14 T, measured in a CsV3_3Sb4.91_{4.91}Sn0.09_{0.09} sample at varying TT between 5 and 100 K. b, c, Two-band model fits of ρxx(H)\rho_{xx}(H) (b) and ρxy(H)\rho_{xy}(H) (c). Blue circles are data taken at T=5T = 5 K. Yellow lines are fits given by Eqs. (8) and (9).

kFk_{\mathrm{F}} (Å−1^{-1})vFv_{\mathrm{F}} (m/s)τ\tau (s)ll (nm)kFlk_{\mathrm{F}}lξloc\xi_{\mathrm{loc}} (nm)
2D cylinder-shaped Fermi surfacehh0.1842.13×1052.13 \times10^{5}3.7×10−143.7 \times10^{-14}7.8814.56.1×10106.1 \times10^{10}
ee0.1772.05×1052.05 \times10^{5}4,0×10−144,0 \times10^{-14}8.214.56.3×10106.3 \times10^{10}
3D spherical Fermi surfaceshh0.2603.0×1053.0 \times10^{5}3.7×10−143.7 \times10^{-14}11.128.6—
ee0.2502.9×1052.9 \times10^{5}4.0×10−144.0 \times10^{-14}11.629—

Table 3. Physical parameters of CsV3_3Sb4.91_{4.91}Sn0.09_{0.09} derived from fitting of ρxx(H)\rho_{xx}(H) and ρxy(H)\rho_{xy}(H). The Fermi vector (kFk_{\mathrm{F}}), Fermi velocity (vFv_{\mathrm{F}}), relaxation time (τ\tau), mean free path (ll), Ioffe-Regel parameter (kFlk_{\mathrm{F}}l) and localization length (ξloc\xi_{\mathrm{loc}}, only for the quasi-2D case) of the hole-type and electron-type carriers in CsV3_3Sb4.91_{4.91}Sn0.09_{0.09}, derived for quasi-2D and 3D Fermi surface structures (see texts). The effective mass m∗m^* was set to 1.0 mem_{\mathrm{e}} (mem_{\mathrm{e}} is the mass of free electron) in the calculation.

We further elucidate that the 3D metal nature of CsV3_3Sb5−x_{5-x}Snx_x imposes stricter constraints on the influence of disorder. In a mean-field picture, the criterion Eq. (7) with d=3d = 3 (where ξloc\xi_{\mathrm{loc}} diverges at the mobility edge [56]) leads to the understanding that Δ\Delta stays almost unchanged (and spatially uniform) across the critical region at the metal-insulator transition [54]. As such, strong inhomogeneity of Δ\Delta as observed in this work can only emerge in a system on the insulating side of the mobility edge; in practice, distinct fluctuation effect stemming from disorder has been observed in a 3D superconductor which locates inside the Anderson critical region near the mobility edge (with kFl<1k_F l < 1 and notably insulating normal-state resistivity) [57]. The absence of insulating ρxx(T)\rho_{xx}(T) in all CsV3_3Sb5−x_{5-x}Snx_x samples (Supplementary Fig. 3), supplied by the lack of signatures of Altshuler-Aronov-type suppression of the DOS at EFE_F [62] in the STM data (Supplementary Fig. 2), unambiguously implies that these samples are far beyond the mobility edge on the metallic side. We thus conclude that our observation of heterogeneous superconductivity cannot be understood within the BCS framework because the localization effect is too weak to yield these outcomes.

As a closing remark, we mention that there are theoretical proposals considering factors beyond the mean-field picture mentioned above (e.g., mesoscopic fluctuations, Coulomb interaction, etc.) [55, 63]; these models predict that self-organized granularity of superconducting state can occur at a weaker disorder strength compared with the original mean-field results. Nevertheless, our samples are still too conductive with regard to the criterion given by these models (for instance, the residual conductivity of CsV3_3Sb4.91_{4.91}Sn0.09_{0.09} is three orders of magnitude larger than the critical conductance gcFg_{\mathrm{cF}} derived from Eq. (1) in Ref. [63], see contexts therein for details). Hence, our main conclusion of negligible localization effect stays unchanged.

Supplementary Note 15

Origin of pair-breaking scattering revealed by STM

Nonmagnetic impurities with moderate scattering potential can break Cooper pairs and induce in-gap states in an unconventional superconductor with a sign-changing order parameter. In Sn-doped CsV3_3Sb5_5, we did not find notable impurity states inside the gap near the Sn dopants that should be nonmagnetic. However, this does not necessarily mean a conventional pairing in this kagome system, since point-like disorder may not serve as an effective phase-sensitive perturbation of superconductivity in kagome lattices owing to the sublattice character of the electronic states [64]. Alternatively, it is also possible that the scattering potential of Sn substitution is simply too weak to induce any in-gap states [65].

Moreover, we observed sparse vanadium-site defects in these crystals and found that they can induce clear in-gap states near EFE_{\mathrm{F}} in the superconducting state (Supplementary Figure 20, Supplementary Figure 20). Their identity is not yet clear but most likely to be vanadium vacancies. If they are nonmagnetic or weakly magnetic, the pronounced in-gap states near zero energy might be a sign for unconventional pairing. Interestingly, we find that the real-space modulations of the in-gap state are unidirectional; this is because the site-symmetry of the defect on one sublattice is lower than the point group symmetry, thus implying the role of the sublattice degree of freedom. This anisotropy further carries over to the QPI images, resulting in a C2_2-symmetric signal at q2\mathbf{q}_2 at the energy of the bound state (Supplementary Fig. 20c). Note that the direction of this signal at q2\mathbf{q}_2 depends on the atomic site of the sublattices for the defects, and is distinct from the direction of q1\mathbf{q}_1 feature that is associated with the charge stripe.

To elucidate the relationship between these impurity states (green circles in Supplementary Figure 20) and the scattering signals in BQPI, we perform Fourier filter on q2\mathbf{q}_2: the real-space features corresponding to q2\mathbf{q}_2 are strongly confined to the V-site defects (Supplementary Figure 20), and are exactly the same as the standing wave patterns near these defects in the raw dI/dVdI/dV map (marked by red arrows in Supplementary Figure 20), indicating a close correlation between the impurity states and the origin of q2\mathbf{q}_2 signals at EFE_\mathrm{F}.

Then, we masked the areas in the vicinity of the V-site impurities to eliminate their contribution to the total zero-energy residual DOS (Supplementary Figure 20). With this process, the signals at q2\mathbf{q}_2 significantly weaken, whereas those at q1\mathbf{q}_1 still persist (Supplementary Figure 20), indicating that the scattering associated with q1\mathbf{q}_1 is more extended in real space and gives rise to the global finite DOS at EFE_\mathrm{F}. Thus, the pair-breaking effect near the V-site defect is not the main origin of the residual DOS at zero-energy. Furthermore, the Fourier filter result of the q1\mathbf{q}_1 feature (Supplementary Figure 20) displays a negligible correlation with the Sn dopant distribution (Supplementary Figure 20), indicating that pair breaking is more likely caused by scattering off the disorder potential associated with the short-range CDW (rather than the Sn dopant). We stress that while point-like disorder acts as a weak pair breaker for spin-singlet sign-changing superconductivity in the Cs-135 series according to a recent theoretical work [64] (owing to the sublattice degree of freedom), a spatially extended object that mixes electronic states of different sublattices, such as the short-range charge-stripe order in the current case, may generate remarkable pair-breaking scattering [27, 66]. The effectiveness of such scattering potential in producing spatially inhomogeneous Δ\Delta lies in the fact that its correlation length (ξCDW∼6\xi_{\mathrm{CDW}} \sim6-18 nm for x=0.15x = 0.15 [24], potentially larger at x=0.07x = 0.07 and 0.09) is comparable to ξab\xi_{\mathrm{ab}} (≃30\simeq30-40 nm, Supplementary Note 3) [27].

Supplementary Note 16:

Nodeless gap structure in x=0.09x = 0.09 sample determined by BQPI measurement

Energy dependence of the BQPI intensity of CsV3Sb4.91Sn0.09

Supplementary Figure 21. Energy dependence of the BQPI intensity of CsV3Sb4.91Sn0.09\mathrm{CsV}_{3}\mathrm{Sb}_{4.91}\mathrm{Sn}_{0.09}. a, Quasiparticle interference pattern measured at −2-2 mV, outside the superconducting gap, using a normal tip at 20 mK. The colored boxes mark the momentum regions used to extract the BQPI intensities. b, Top panel: representative superconducting spectrum acquired under the same conditions. Bottom panel: energy dependence of the BQPI intensity at different scattering wavevectors marked in a. The BQPI intensities are strongly suppressed inside the superconducting gap, as expected from the depletion of quasiparticle spectral weight after gap opening. c, d, Same measurements and analysis as in a and b, but acquired using a superconducting Nb tip at 320 mK. In both datasets, the BQPI intensity is suppressed in all selected momentum regions upon entering the superconducting gap, indicating that the corresponding electronic states become gapped in the superconducting state. These results support a nodeless superconducting gap on the detected Fermi-surface sections of CsV3Sb4.91Sn0.09\mathrm{CsV}_{3}\mathrm{Sb}_{4.91}\mathrm{Sn}_{0.09}.

Possible scenarios of the sign-reversal superconducting pairing

The possibility that unconventional superconducting states emerge in a kagome lattice has been extensively investigated in existing theoretical efforts [51, 52, 67, 68, 69, 70, 71, 72, 73]. Surprisingly rich superconducting phase diagrams have been proposed for kagome superconductors, owing to their unique properties of (i) specific sublattice interference, (ii) appreciable intersite Coulomb interactions and (iii) the presence of multiple van Hove singularities in the vicinity of EFE_{\mathrm{F}} [51, 52, 67, 68, 69]. Considering the point group C6vC_{6v} of a 2D kagome lattice, the allowed pairing symmetries correspond to the irreps A1A_{1}, A2A_{2} (spin-singlet), B1B_{1}, B2B_{2}, E1E_{1} (spin-triplet) and E2E_{2} (spin-singlet); here we focus on the most representative candidates of unconventional gap functions:

  1. The chiral triplet pp-wave order (p+ipp+ip, E1E_{1} irrep), see main text Fig. 5a,

  1. The chiral singlet dd-wave order (d+idd+id, E2E_{2} irrep), see main text Fig. 5b.

Both (1) and (2) are time-reversal symmetry breaking (TRSB) and nodeless (i.e., exhibiting a fully-opened superconducting gap); both can be the leading pairing instabilities in kagome lattices under certain circumstances [52, 68, 69]. If the inter-sublattice interaction becomes dominant, a (3) nodal ff-wave triplet pairing state (irreps B1B_{1} or B2B_{2}, the latter shown in main text Fig. 5c) can be promoted [51, 52, 68, 69]. Alternatively, if the electron-phonon coupling of the Sb pp orbital (Fermi surface centered at the Γ\Gamma point of the first Brillouin zone, distinguished from the hexagonal Fermi surfaces of the kagome V 3d3d electrons) is highlighted, the most likely scenarios of superconducting pairing include (4) a sign-changing s+−s^{+-} state (illustrated in main text Fig. 5d) [70].

Among pairing symmetries (1)-(4), we suggest that (3) can be largely precluded, because the ff-wave superconductivity is nodal [51, 52, 68, 69] with gap zeros occurring on the hexagonal Fermi surface along specific directions (Γ\Gamma-K for the B2B_{2} state in main text Fig. 5c), whereas our STM results demonstrate the absence of corresponding gap nodes (see Supplementary Note 16). Moreover, the most relevant scattering vectors (arrows in main text Fig. 5) inferred from the QPI analysis (main text Fig. 4) connect Fermi surface sections with the same sign of the superconducting order parameter for the ff-wave pairing (main text Fig. 5c), thus become less effective in breaking Cooper pairs. The chiral pp-wave state (1) is also less likely, since the triplet pairing ought to be sensitive to point-like disorder [64] and hence yield a prominent pair-breaking effect at the Sn dopants, which is not observed in our STM experiments (Supplementary Note 15).

The remaining two possibilities, i.e., (2) d+idd+id (main text Fig. 5b) and (4) s+−s^{+-} (main text Fig. 5d) pairing states, are more realistic for Cs-135 kagome superconductors [70] and both can explain our main observations at the qualitative level. As illustrated in main text Fig. 5b, the d+idd+id gap function shows a phase winding around the hexagonal Fermi surface, Δ(φ)=Δexp⁡(i2φ)\Delta(\varphi)=\Delta\exp(i2\varphi) (φ\varphi is the polar angle with respect to the xx direction) [71]. Consequently, the scattering process at vector q1\mathbf{q}_{1} involves Fermi surfaces with remarkable phase shifts of the superconducting order parameter (main text Fig. 5b, except for the k→−k\mathbf{k}\rightarrow-\mathbf{k} scattering denoted by the black arrow), effectively resulting in the breaking of Cooper pairs (note that the k→−k\mathbf{k}\rightarrow-\mathbf{k} scattering induced by point-like impurities is only weakly pair-breaking [64]). For the s+−s^{+-}-wave pairing (main text Fig. 5d), the Fermi surface segments connected by q1\mathbf{q}_{1} host superconducting gap with the same sign, whilst the pair-breaking scattering may occur between the original and folded Fermi surfaces in the presence of charge-stripe order (red arrow in main text Figure 5d); note that the folded bands produced by the λ∼3a0\lambda\sim3a_0 stripe order are close to the pp-orbital Fermi surface located at Γ\Gamma (main text Figure 4e and Supplementary Figure 15), therefore, Δ\Delta at these momenta might change its sign relative to the original kagome bands due to the pp-dd hybridization.

To seek possible phase-sensitive evidence for such sign-changing pairing states, we further performed magnetic-field-dependent and phase-referenced QPI analyses (Supplementary Fig. 22). The dominant scattering vectors resolved in the QPI measurements are summarized schematically in Supplementary Fig. 22a, and the corresponding experimental QPI pattern measured at 2 mV is shown in Supplementary Fig. 22d. Their relation to two representative candidate pairing states, chiral d+idd+id and s±s_{\pm}, is illustrated in Supplementary Fig. 22b and c. Following Ref. [74], we examined the field-induced QPI change, defined as δg(q,E,0.1T)=g(q,E,0.1T)−g(q,E,0T)\delta g(\mathbf{q},E,0.1\mathrm{T})=g(\mathbf{q},E,0.1\mathrm{T})-g(\mathbf{q},E,0\mathrm{T}), where sign-preserving and sign-reversing scattering channels are expected to respond differently to magnetic field. As displayed in Supplementary Fig. 22e-h, the field-induced QPI changes at representative in-gap energies are dominated by positive contrast, and no well-defined field-suppressed feature can be assigned to a sign-reversing scattering channel. To assess the possible influence of the set-point effect, we constructed conductance-ratio maps Z(r,E)=g(r,+E)/g(r,−E)Z(\mathbf{r},E)=g(\mathbf{r},+E)/g(\mathbf{r},-E) for the x=0.09x=0.09 sample. As shown in Supplementary Fig. 22i-l, the in-gap QPI features are too weak for a reliable field-dependent analysis. The origin of this weak QPI contrast remains unclear. Previous QPI/BQPI studies of the superconducting state in CsV3_3Sb5_5-based systems have also primarily analyzed g(q,E)g(\mathbf{q},E) maps [45, 75]. Moreover, the normal-state conductance and integrated low-energy DOS in our x=0.09x=0.09 sample show weak spatial variations (Fig. 3 and Supplementary Fig. 2), suggesting that spatial variations in the set-point normalization may be limited. We therefore retain the g(q,E)g(\mathbf{q},E) maps to examine the field response of the resolved QPI channels.

We also calculated the phase-referenced QPI signal based on the complex FT-QPI signal g(q,E)=∣g(q,E)∣eiφ(q,E)g(\mathbf{q},E)=|g(\mathbf{q},E)|e^{i\varphi(\mathbf{q},E)}, where φ(q,E)\varphi(\mathbf{q},E) is the Fourier phase. The phase-referenced signal is defined as gPR(q,E)=∣g(q,+E)∣cos⁡[φ(q,+E)−φ(q,−E)]g_{\mathrm{PR}}(\mathbf{q},E)=|g(\mathbf{q},+E)|\cos[\varphi(\mathbf{q},+E)-\varphi(\mathbf{q},-E)], for which sign-reversing scattering channels are expected to give negative contrast [76, 77, 78]. As shown in Supplementary Fig. 22m-p, the phase-referenced QPI maps of our data are also dominated by positive contrast, without a well-defined negative signal localized at the relevant QPI vectors. Thus, neither magnetic-field-dependent QPI nor phase-referenced QPI provides direct evidence for sign-reversing scattering channels in the present data.

The absence of such a phase-sensitive QPI signature does not rule out a momentum-dependent phase structure of the superconducting order parameter; instead, it can be attributed to the nature of the QPI channels resolved in CsV3_3Sb5−x_{5-x}Snx_x. The predominant QPI features in our measurements are mostly intra-pocket scatterings, rather than inter-pocket scatterings connecting two known opposite-sign momenta (which is the case for the previous successful applications of phase-sensitive QPI analysis for high-Tc superconductors). In Supplementary Fig. 22b and c, we illustrate this issue for the two most likely pairing symmetries, i.e., d+idd+id and s±s_{\pm}, respectively; the black double arrow q1\mathbf{q}_1 denote the predominant intra-pocket scattering vector that is captured by our QPI measurements, which does not connect Fermi surface regions with opposite signs of the superconducting order parameter. For complex pairing states such as chiral d+idd+id or chiral p+ipp+ip, or for the possible s±s^{\pm} scenario discussed above, the dominant in-gap QPI signal q1\mathbf{q}_1 does not necessarily connect Fermi-surface regions with opposite signs of the superconducting order parameter (Supplementary Fig.) 22b and c). Therefore, the present QPI data do not provide direct phase information or unambiguous evidence for sign-reversal pairing; determination of the exact superconducting phase structure will require future phase-sensitive experiments and theoretical modelling.

Magnetic-field-dependent and phase-referenced QPI analyses

Figure 22. Schematic Fermi surface and main scattering vectors resolved in the QPI measurements. b, c, Illustrations of chiral dd-wave (d+idd+id) pairing state (b) and the s±s^{\pm}-wave pairing state (c). The double-arrow vectors q1\mathbf{q}_1 correspond to those shown in a. d, Experimental QPI pattern measured at 2 mV, showing the dominant scattering features q1\mathbf{q}_1 and q2\mathbf{q}_2. e-h, Magnetic-field-induced QPI changes δg(q,E,0.1 T)\delta g(\mathbf{q}, E, 0.1\ \mathrm{T}) at representative in-gap energies. The field-induced signals are predominantly positive; no clear field-suppressed feature can be resolved at the relevant QPI vectors. i, j Fourier-transformed Z(q,E)Z(\mathbf{q}, E) maps of the x=0.09x=0.09 sample measured at 0 T, with E=70E=70 and 140 μeV\mu\mathrm{eV} respectively. k, l, Corresponding Z(q,E)Z(\mathbf{q}, E) maps measured at 0.1 T. The QPI features in these ZZ maps are too weak for a reliable field-dependent comparison m-p, Phase-referenced QPI maps gPR(q,E)g_{\mathrm{PR}}(\mathbf{q}, E) at representative in-gap energies. The phase-referenced signals are also dominated by positive contrast, without a well-defined negative signal localized at the relevant QPI vectors.

We emphasize that these arguments presented above are completely qualitative and phenomenological. The exact pairing symmetry of superconducting states in charge-stripe ordered CsV3Sb5−xSnx\mathrm{CsV}_{3}\mathrm{Sb}_{5-x}\mathrm{Sn}_{x} will only be nailed down in future studies exploiting new phase-sensitive techniques. Some theoretical proposals [72, 73] also predict the formation of pair density wave (PDW) order in kagome lattices, which possesses Cooper pairs characterized by specific finite momentum qq and may have intricate connections with the CDW order in the normal state. Nevertheless, we also mention that the unusual superconducting state in CsV3Sb5−xSnx\mathrm{CsV}_{3}\mathrm{Sb}_{5-x}\mathrm{Sn}_{x} (x=0.09x = 0.09) can hardly be associated with the PDW state as discussed in the main text.

References

  1. [1]Oey, Y. M. et al. Fermi level tuning and double-dome superconductivity in the kagome metal CsV₃Sb₅₋ₓSnₓ. Phys. Rev. Mater. 6, L041801 (2022).
  2. [2]Kongruengkit, T. et al. Persistence of charge density wave fluctuations in the absence of long-range order in a hole-doped kagome metal. Phys. Rev. Mater. 10, L022001 (2026).arxiv.org/abs/2508.13290
  3. [3]Tinkham, M. Introduction to Superconductivity. Dover Books on Physics Series (Dover Publications, 2004).
  4. [4]Ortiz, B. R. et al. CsV₃Sb₅: a Z₂ topological kagome metal with a superconducting ground state. Phys. Rev. Lett. 125, 247002 (2020).
  5. [5]Maza, J. & Vidal, F. Critical-temperature inhomogeneities and resistivity rounding in copper oxide superconductors. Phys. Rev. B 43, 10560 (1991).pubmed.ncbi.nlm.nih.gov/9996783
  6. [6]Larkin, A. & Varlamov, A. A. Theory of Fluctuations in Superconductors (Oxford University Press, Oxford, 2005).DOI
  7. [7]Halperin, B. I. & Nelson, D. R. Resistive transition in superconducting films. J Low Temp Phys 36, 599-616 (1979).DOI
  8. [8]Rullier-Albenque, F., Alloul, H. & Rikken, G. High-field studies of superconducting fluctuations in high-Tc cuprates: Evidence for a small gap distinct from the large pseudogap. Phys. Rev. B 84, 014522 (2011).
  9. [9]Caprara, S., Grilli, M., Leridon, B. & Lesueur, J. Extended paraconductivity regime in underdoped cuprates. Phys. Rev. B 72, 104509 (2005).DOI
  10. [10]Kasahara, S. et al. Giant superconducting fluctuations in the compensated semimetal FeSe at the BCS-BEC crossover. Nat. Commun. 7, 12843 (2016).DOI
  11. [11]Oganesyan, V., Huse, D. A. & Sondhi, S. L. Theory of diamagnetic response of the vortex liquid phase of two-dimensional superconductors. Phys. Rev. B 73, 094503 (2006).DOI
  12. [12]Yu, G. et al. Universal precursor of superconductivity in the cuprates. Phys. Rev. B 99, 214502 (2019).
  13. [13]Popčević, P. et al. Percolative nature of the direct-current paraconductivity in cuprate superconductors. npj Quantum Mater. 3, 42 (2018).DOI
  14. [14]Pelc, D. et al. Emergence of superconductivity in the cuprates via a universal percolation process. Nat. Commun. 9, 4327 (2018).DOI
  15. [15]Pelc, D. et al. Unusual behavior of cuprates explained by inhomogeneous charge localization. Sci. Adv. 5, eaau4538 (2019).DOI
  16. [16]Torrón, C., Díaz, A., Pomar, A., Vieira, J. A. & Vidal, F. Measurements of fluctuation-induced diamagnetism above the superconducting transition in YBa₂Cu₃O₇₋δ single crystals in low magnetic fields: Comparison with paraconductivity, Phys. Rev. B 49, 13143 (1994).pubmed.ncbi.nlm.nih.gov/10010230
  17. [17]Viña, J. et al. Universal behavior of the in-plane paraconductivity of cuprate superconductors in the short-wavelength fluctuation regime. Phys. Rev. B 65, 212509 (2002).
  18. [18]Caprara, S., Grilli, M., Benfatto, L. & Castellani, C. Effective medium theory for superconducting layers: a systematic analysis including space correlation effects. Phys. Rev. B 84, 014514 (2011).DOI
  19. [19]Benfatto, L., Toschi, A., Caprara, S. & Castellani, C. Coherence length in superconductors from weak to strong coupling. Phys. Rev. B 66, 054515 (2002).DOI
  20. [20]Ghosal, A., Randeria, M. & Trivedi, N. Role of spatial amplitude fluctuations in highly disordered s-wave superconductors. Phys. Rev. Lett. 81, 3940 (1988).
  21. [21]Bouadim, K., Loh, Y. L., Randeria, M. & Trivedi, N. Single-and two-particle energy gaps across the disorder-driven superconductor–insulator transition. Nat. Phys. 7, 884-889 (2011).DOI
  22. [22]Maccari, I., Benfatto, L., & Castellani, C. Broadening of the Berezinskii-Kosterlitz-Thouless transition by correlated disorder. Phys. Rev. B, 96, 060508(R) (2017).DOI
  23. [23]Kresin, V. Z., Ovchinnikov, Y. N. & Wolf, S. A. Inhomogeneous superconductivity and the “pseudogap” state of novel superconductors. Phys. Rep. 431, 231 (2006).
  24. [24]Kautzsch, L. et al. Incommensurate charge-stripe correlations in the kagome superconductor CsV₃Sb₅-xSnₓ. npj Quantum Mater. 8, 37 (2023).DOI
  25. [25]Huai, L. et al. Electron-Correlation-Assisted Charge Stripe Order in a Kagome Superconductor. Phys. Rev. X 15, 041039 (2025).arxiv.org/abs/2509.17467
  26. [26]Spivak, B., Oreto, P. & Kivelson, S. A. A Theory of quantum metal to superconductor transitions in highly conducting systems. Phys. Rev. B 77, 214523 (2008).DOI
  27. [27]Dodaro, J. F. & Kivelson, S. A. Generalization of Anderson's theorem for disordered superconductors. Phys. Rev. B 98, 174503 (2018).DOI
  28. [28]Li, Z.-X., Kivelson, S. A. & Lee, D.-H. Superconductor-to-metal transition in overdoped cuprates. npj Quantum Mater. 6, 36 (2021).arxiv.org/abs/2010.06091
  29. [29]Deng, L. et al. Ambient-pressure 151-K superconductivity in HgBa2Ca2Cu3O8+δ via pressure quench. Proc. Natl Acad. Sci. USA 123, e2536178123 (2026).DOI
  30. [30]Luo, Y. et al. A unique van Hove singularity in kagome superconductor CsV₃-xTaxSb₅ with enhanced superconductivity. Nat. Commun. 14, 3819 (2023).DOI
  31. [31]Padamsee, H., Neighbor, J. E. & Shiffman, C. A. Quasiparticle Phenomenology for Thermodynamics of Strong-Coupling Superconductors. J. Low Temp. Phys. 12, 387 (1973).DOI
  32. [32]Johnston, D. C. Elaboration of the α-model derived from the BCS theory of superconductivity, Supercond. Sci. Technol. 26, 115011 (2013).DOI
  33. [33]Gupta, R. et al. Microscopic evidence for anisotropic multigap superconductivity in the CsV₃Sb₅ kagome superconductor. npj Quantum. Mater. 7, 49 (2022).DOI
  34. [34]Roppongi, M. et al. Bulk evidence of anisotropic s-wave pairing with no sign change in the kagome superconductor CsV₃Sb₅. Nat Commun. 14, 667 (2023).DOI
  35. [35]Sun, Y. et al. Imaging momentum-space Cooper pair formation and its competition with the charge density wave gap in a kagome superconductor, Sci. China Phys. Mech. Astron. 67, 277411 (2024).DOI
  36. [36]Xu, H.-S. et al. Multiband superconductivity with sign-preserving order parameter in kagome superconductor CsV₃Sb₅. Phys. Rev. Lett. 127, 187004 (2021).DOI
  37. [37]Duan, W. et al. Nodeless superconductivity in the kagome metal CsV₃Sb₅. Sci. China Phys. Mech. Astron. 64, 107462 (2021).DOI
  38. [38]Clem, J. R. Effects of Energy Gap Anisotropy in Pure Superconductors. Ann. Phys. (N.Y.) 40, 268 (1966).DOI
  39. [39]Nakajima, Y., Nakagawa, T., Tamegai, T. & Harima, H. Specific-Heat Evidence for Two-Gap Superconductivity in the Ternary-Iron Silicide Lu₂Fe₃Si₅. Phys. Rev. Lett. 100, 157001 (2008).pubmed.ncbi.nlm.nih.gov/18518144
  40. [40]Hardy, F. et al. Multiband Superconductivity in KFe₂As₂: Evidence for One Isotropic and Several Lilliputian Energy Gaps. J. Phys. Soc. Jpn. 83, 014711 (2014).DOI
  41. [41]Guritanu, V., Goldacker, W., Bouquet, F., Wang, Y., Lortz, R, Goll, G. & Junod, A. Specific heat of Nb₃Sn: The case for a second energy gap. Phys. Rev. B 70, 184526 (2004).DOI
  42. [42]Chen, G.-Y., Zhu, X., Yang, H. & Wen, H. H. Highly anisotropic superconducting gaps and possible evidence of antiferromagnetic order in FeSe single crystals. Phys. Rev. B 96, 064524 (2017).DOI
  43. [43]Tallon, J. L., Storey, J. G. & Loram, J. W.Fluctuations and critical temperature reduction in cuprate superconductors. Phys. Rev. B 83, 092502 (2011).DOI
  44. [44]Tallon, J. L. Barber, F., Storey, J. G. & Loram, J. W. Coexistence of the superconducting energy gap and pseudogap above and below the transition temperature of cuprate superconductors. Phys. Rev. B 87, 140508(R) (2013).DOI
  45. [45]Wu, P. et al. Unidirectional electron-phonon coupling in the nematic state of a kagome superconductor. Nat. Phys. 19, 1143 (2023).DOI
  46. [46]Zhong, Y. et al. Nodeless electron pairing in CsV₃Sb₅-derived Kagome superconductors. Nature 617, 488-492 (2023).DOI
  47. [47]Superconductivity, edited by R. D. Parks (Marcel Dekker, New York, 1969).
  48. [48]Wang, Y., Yan, J., Shan, L., Wen, H.-H., Tanabe, Y., Adachi, T. & Koike, Y. Weak-coupling d-wave BCS superconductivity and unpaired electrons in overdoped La₂₋ₓSrₓCuO₄ single crystals. Phys. Rev. B 76, 064512 (2007).DOI
  49. [49]Mu, G. et al. Sizable Residual Quasiparticle Density of States Induced by Impurity Scattering Effect in Ba(Fe₁₋ₓCoₓ)₂As₂ Single Crystals. Chin. Phys. Lett. 27, 037402 (2010).
  50. [50]Wade, J. M., Loram, J. W., Mirza, K. A., Cooper, J. R. & Tallon, J. L. Electronic Specific Heat of Tl₂Ba₂CuO₆+δ from 2 K to 300 K for 0≤δ≤0.1. J. Supercond. 7, 261 (1994).DOI
  51. [51]Ding, P., Lee, C. H., Wu, X. & Thomale, R. Diagnosis of pairing symmetry by vortex and edge spectra in kagome superconductors. Phys. Rev. B 105, 174518 (2022).DOI
  52. [52]Wu, X., Chakraborty, D., Schnyder, A. P. & Greco, A. Crossover between electron-electron and electron-phonon mediated pairing on the kagome lattice. Phys. Rev. B 109, 014517 (2024).DOI
  53. [53]Ikuta, H., Matsuura, M. & Biwa, T. Low-temperature specific heat of overdoped Bi₂₂₀₁ single crystals. Physica C 388-389, 361-362 (2003).
  54. [54]Ma, M. & Lee, P. A. Localized superconductors. Phys. Rev. B 32, 5658 (1985).pubmed.ncbi.nlm.nih.gov/9937812
  55. [55]Feigel'man, M. V., Ioffe, L. B., Kravtsov, V. E. & Cuevas, E. Fractal superconductivity near localization threshold. Ann. Phys. (N.Y). 325, 1390 (2010).
  56. [56]Lee, P. A. & Ramakrishnan, T. V. Disordered electronic systems. Rev. Mod. Phys. 57, 287 (1985).
  57. [57]Qi, S. et al. Quantum Griffiths Singularity in a Three-Dimensional Superconductor to Anderson Critical Insulator Transition. Phys. Rev. Lett. 133, 226001 (2024).DOI
  58. [58]Kagawa, K., Inagaki, K. & Tanda, S. Superconductor-insulator transition in ultrathin Pb films: Localization and superconducting coherence. Phys. Rev. B 53, R2979 (1996).pubmed.ncbi.nlm.nih.gov/9983900
  59. [59]Sambandamurthy, G., Das Gupta, K. & Chandrasekhar, N. Effect of granularity on the insulator-superconductor transition in ultrathin Bi films. Phys. Rev. B 64, 014506 (2001).DOI
  60. [60]Liu, S. et al. Impact of Tiny Fermi Pockets with Extremely High Mobility on the Hall Anomaly in the Kagome Metal CsV₃Sb₅. Phys. Rev. Lett. 135, 056502 (2025).DOI
  61. [61]Ashcroft, N. W. & Mermin, N. D. Solid State Physics (Harcourt, Orlando, 1976).
  62. [62]Carbillet, C. et al., Spectroscopic evidence for strong correlations between local superconducting gap and local Altshuler-Aronov density of states suppression in ultrathin NbN films. Phys. Rev. B 102, 024504 (2020).DOI
  63. [63]Skvortsov, M. A. & Feigel’man, M. V. Superconductivity in Disordered Thin Films - Giant Mesoscopic Fluctuations. Phys. Rev. Lett. 95, 057002 (2005).DOI
  64. [64]Holbæk, S. C., Christensen, M. H., Kreisel, A. & Andersen, B. M. Unconventional superconductivity protected from disorder on the kagome lattice. Phys. Rev. B 108, 144508 (2023).DOI
  65. [65]Yang, H. et al. Unexpected weak spatial variation in the local density of states induced by individual Co impurity atoms in superconducting Na(Fe₁-xCoₓ)As crystals revealed by scanning tunneling spectroscopy. Phys. Rev. B 86, 214512 (2012).
  66. [66]Gannot, Y., Ramshaw, B. J. & Kivelson, S. A. Fermi surface reconstruction by a charge density wave with finite correlation length. Phys. Rev. B 100, 045128 (2019).DOI
  67. [67]Wang, W.-S. Li, Z.-Z., Xiang, Y.-Y. & Wang, Q.-H. Competing electronic orders on kagome lattices at van Hove filling. Phys. Rev. B 87, 115135 (2013).DOI
  68. [68]Wu, X., et al. Nature of Unconventional Pairing in the Kagome Superconductors AV₃Sb₅ (A = K, Rb, Cs). Phys. Rev. Lett. 127, 177001 (2021).DOI
  69. [69]Rømer, A. T. Bhattacharyya, S., Valentí, R., Christensen, M. H. & Andersen, B. M. Superconductivity from repulsive interactions on the kagome lattice. Phys. Rev. B 106, 174514 (2022).
  70. [70]Ritz, E. T., Røising, H. S., Christensen, M. H., Birol, T., Andersen, B. M. & Fernandes, R. M. Superconductivity from orbital-selective electron-phonon coupling in AV₃Sb₅. Phys. Rev. B 108, L100510 (2023).DOI
  71. [71]Nandkishore, R., Levitov, L. S. & Chubukov, A. V. Chiral superconductivity from repulsive interactions in doped graphene. Nat. Phys. 8, 158 (2012).DOI
  72. [72]Jin, J.-T., Jiang, K., Yao, H. & Zhou, Y. Interplay between Pair Density Wave and a Nested Fermi Surface. Phys. Rev. Lett. 129, 167001 (2022).DOI
  73. [73]Wu, Y.-M., Thomale, R. & Raghu, S. Sublattice interference promotes pair density wave order in kagome metals. Phys. Rev. B 108, L081117 (2023).arxiv.org/abs/2211.01388
  74. [74]Hanaguri, T., Niitaka, S, Kuroki, K. & Takagi, H. Unconventional s-wave superconductivity in Fe(Se,Te). Science 328, 474 (2010).DOI
  75. [75]Greenberg, A. G. et al. Momentum structure of superconductivity and sublattice effects from quasiparticle interference in CsV₃Sb₅. arXiv 2607.27148 (2026).arxiv.org/abs/2607.27148
  76. [76]Chi, S. et al. Extracting phase information about the superconducting order parameter from defect bound states. arXiv:1710.09088 (2017).arxiv.org/abs/1710.09088
  77. [77]Gu, Q. et al. Directly visualizing the sign change of d-wave superconducting gap in Bi₂Sr₂CaCu₂O₈+δ by phase-referenced quasiparticle interference. Nat. Commun. 10, 1603 (2019).
  78. [78]Gu, Q. et al. Sign-reversal superconducting gaps revealed by phase-referenced quasiparticle interference of impurity-induced bound states in (Li₁−xFeₓ)OHFe₁−yZnᵧSe. Phys. Rev. B 98, 134503 (2018).DOI

Paper details

vlnc:W_zwm8q5gr
Version
v1 · latest
Published
Fresh — added to the Hub within the last 30 days
Added
License
CC BY 4.0
Usage

views · 6

downloads · 0

A view counts once per browser per day, a download each time the PDF is requested.

  • Physics and Astronomy

Not recorded for this paper

View statement
Looking for related papers…
Contents