WorksPhysics and Astronomy
Tunable Itinerant Ferromagnetism in the Two-Dimensional FePdTe Hosting 1D Spin Chains
Abstract
One-dimensional (1D) magnetism offers unidirectional spin interactions that allow unique tunable properties and unconventional spin phenomena. However, it often suffers from poor stability, limiting practical applications. In this regard, integrating 1D magnetism into two-dimensional (2D) materials enables a promising route to stabilize these systems while preserving their anisotropic magnetic characteristics. Here, we focus on the 2D ferromagnet FePdTe (T = 183K), which hosts 1D spin chains and strong in-plane anisotropy. Our first-principles calculations reveal highly anisotropic magnetic exchange interactions, confirming its 1D ferromagnetic nature. We modulate this behavior by Co and Ni substitution and introduce two new members of this family, CoPdTe – a ferromagnet – and NiPdTe. Our results unveil the microscopic mechanisms governing the behaviour of FePdTe and CoPdTe. Furthermore, we also demonstrate that the variation of the chain length is key to modulate magnetism. Finally, we determine the magnon dispersion, showcasing a pronounced anisotropy that enables unidirectional magnon propagation.
The discovery of intrinsic magnetism in two-dimensional (2D) systems has revolutionized the fields of condensed matter, thin-films chemistry and material science, positioning 2D van der Waals (vdW) magnets as promising candidates for next-generation quantum technologies.[1, 2, 3]
To date, a wide variety of 2D magnetic materials with a broad range of electronic and magnetic properties has been reported, including antiferromagnetic (AF) semiconductors such as CrSBr, CrI and the MPS family,[4, 5, 6, 7] or the metallic ferromagnets FeGaTe and FeGeTe (x = 3, 4, 5).[8, 9, 10, 11, 12] Most of these systems exhibit symmetric arrangements of their magnetic centres, leading to spin-spin interactions in different directions and thus limiting the unidirectional control over their magnetic properties.[13, 14] In this context, one-dimensional (1D) magnetism offers a compelling route to localize magnetism by minimizing interactions between neighbouring spins, allowing the emergence of exotic phenomena.[15, 16, 17, 18] However, the practical isolation of materials hosting individual 1D spin chains possesses a major challenge, mainly due to their poor stability and fabrication complexity.[19, 20] Thus, the rational design of novel 2D magnets that combine the strong anisotropy of 1D spin chains with the ultrathin 2D nature of these systems is of great scientific interest.
A prominent example of this class of systems is AgCrPS,[21, 22] an anisotropic vdW antiferromagnet (T = 21K) that shares structural similarities with the MPS family.[14, 23] Unlike the honeycomb magnetic lattice in MPS, AgCrPS contains Cr atoms forming well-isolated 1D zigzag chains separated by non-magnetic Ag atoms, thus leading to a 1D magnetic behaviour within each layer. More recently, FePdTe has positioned as a promising 2D vdW magnet hosting 1D spin chains, owing to its ferromagnetic (FM) order with a relatively high T of 183K.[24] This 2D material crystallizes in a layered structure with Fe atoms forming zigzag chains along the crystallographic b-axis, displaying metallic conductivity. Additionally, it shows strong in-plane uniaxial magnetic anisotropy and a large coercive field, highlighting its potential for spintronics and magnonics applications.
One of the key advantages of low-dimensional magnetic materials is their tunability, as external perturbations such as strain or chemical doping can strongly influence their magnetic behaviour.[25, 26, 27, 28] For instance, Co doping in modulates its magnetic anisotropy and pins domain walls,[29] while in it induces a transition from itinerant ferromagnetism to antiferromagnetism, accompanied by a reduction of its critical temperature.[30] Similarly, in , Co substitution raises its , reorients easy axis of magnetization, and triggers a transition from FM to AF order.[31, 32] In , Co doping also drives an AF-FM transition, ultimately leading to a spin glass state, the latter also observed upon addition of Ni atoms.[33, 34]
Therefore, given the potential of as a host for 1D spin chains, combined with the proven effectiveness of Co and Ni doping in tuning the magnetic properties of Fe-based metallic ferromagnets, a detailed investigation of the magnetic properties of along with the impact Co and Ni substitution deserves urgent attention.
In this work, we employ first-principles calculations to investigate the electronic and magnetic properties of , unveiling the 1D nature of its exchange interactions and the mechanisms stabilizing its long-range ferromagnetism. We demonstrate that doping with Co and Ni atoms effectively tunes its magnetic properties, predict the dynamical stability of the isostructural and compounds and explore the potential of strain engineering to modulate their magnetic behaviour. Finally, we determine the magnon dispersion of and , showing that the pronounced anisotropy in their magnon spectra supports unidirectional propagation of magnons along their 1D spin chains.
FePdTe is a recently synthesized quasi-2D crystal, which possesses 1D Fe zigzag chains along the crystallographic axis and a relatively high of 183 K.[24] It displays a monoclinic symmetry within the P2/m (No. 11) space group and lattice parameters of Å, Å, Å, , and (see Figure 1a). Firstly, we perform density-functional theory (DFT) calculations on FePdTe, obtaining optimized lattice parameters of Å, Å, Å, and , and , with a distance between adjacent 1D spin chains of 7.96 Å, in good agreement with experimental results. The computed magnetic moment for each Fe atom is 2.75 , closely matching the reported value of 2.83 for a single domain crystal,[24] while Pd and Te atoms exhibit null spin polarization. From the calculation of the electronic band structure, one can observe that the system is metallic (Figure 1c), with d orbitals of Fe playing a crucial role around the Fermi level and a significant contribution of d and p orbitals of Pd and Te atoms, respectively (Figure S1). The dynamic stability of bulk FePdTe is assessed by performing phonon calculations. As observed in Figure 1d, the phonon dispersion presents no imaginary frequencies, indicating that the structure is stable.
Figure 1. (a) Top view of bulk . Color code: Fe (red), Pd (grey) and Te (green). (b) 3D Brillouin zone (BZ) of and illustration of 1D chain of the material. (c) Band structure and (d) phonon spectra for , and (from left to right, respectively).
Additionally, we calculated its formation energy () using the following expression[35]:
where is the energy of FePdTe and , and represent the energies of isolated Fe, Pd and Te atoms. We obtain eV/atom, indicating that the system is stable.
Furthermore, we investigated the structural, electronic and magnetic properties of bulk isostructural CoPdTe and NiPdTe. Both materials retain the monoclinic symmetry. The optimized lattice parameters of CoPdTe are Å, Å, Å, , and , whereas for NiPdTe they are Å, Å, Å, , and . Our results reveal that CoPdTe does possess a FM ground state, with each Co atom carrying a magnetic moment of . Conversely, NiPdTe is paramagnetic. This is equivalent to the behaviour of NiGeTe ( and ), which exhibits temperature-independent paramagnetism, in contrast to the itinerant ferromagnetism observed in FeGeTe.[36, 37] Regarding the electronic properties, the band structure evidences that both CoPdTe and NiPdTe display a metallic behaviour. Similar to FePdTe, the orbitals of Co and Ni atoms contribute significantly near the Fermi level (Figures S2-Figure 3). Then, we assess their dynamical stability by means of their phonon spectra, which reveal no imaginary frequencies for CoPdTe and a small negative contribution around for NiPdTe (Figure 1d). Moreover, they exhibit values of eV/atom and eV/atom, respectively, which are comparable to that of FePdTe, indicating the feasibility of synthesizing those compounds.

Figure 3. Top view of D chains in the ALT configuration for (a) and (a) along with their corresponding (c) magnetic couplings for each material. Top view of D chains in the CON configuration for (d) and (e) along with their corresponding (f) magnetic couplings for each material.
Subsequently, we calculate the magnetic anisotropy energy (MAE) of FePdTe and CoPdTe from the total energy difference for spin orientations along the , , and directions. In agreement with experimental results, FePdTe presents uniaxial anisotropy, with the easy axis of magnetization oriented along the in-plane direction. The and directions correspond to intermediate and hard axes, exhibiting MAE values of meV/Fe and meV/Fe, respectively. For CoPdTe, the magnetization aligns along the direction, and the intermediate and hard axes are reversed relative to FePdTe, with corresponding MAE values of meV/Co along and meV/Co along .
Next, we derive the magnetic exchange interactions for FePdTe and CoPdTe using a spin Hamiltonian with the following form:
where denotes the isotropic exchange interaction between magnetic moments and , and represents the single-ion magnetic anisotropy constant.
The magnetic interaction picture in FePdTe and CoPdTe can be described by two primary in-plane contributions: (i) inter-site interactions between Fe and Fe sites, denoted as , and (ii) interactions between equivalent magnetic centres, Fe–Fe, labelled as . In constructing the spin Hamiltonian, the selected couplings are considered as a function of distance up to a maximum of 14 Å, beyond which they vanish. Analysing , we observe that both FePdTe and CoPdTe exhibit FM behaviour (Figure 2c). Specifically, FePdTe displays a value of 32.8 meV, which is reduced to 11.6 meV in its Co counterpart. In FePdTe, the strong FM character of is primarily governed by the -, -, -, - and - orbitals (Figure 2d). This FM behaviour is partially diminished by AF contributions from - and - orbitals. For CoPdTe, the FM nature of is attributed to the contribution of - and - orbitals. Figure 2d illustrates the difference in the orbital-resolved contribution to () between both materials, obtained by subtracting the contribution of CoPdTe from FePdTe. This reveals that the enhanced ferromagnetism in FePdTe arises from stronger FM character of -, - and - relative to CoPdTe. A distinct trend is observed for between both systems (Figure 2c). In CoPdTe, is FM, whereas in FePdTe it is AF, primarily due to contributions of - orbitals (Figure 2e). The coexistence of competing FM and AF interactions in FePdTe leads to a geometrically frustrated spin system, thereby partially suppressing the net ferromagnetism within the lattice, similar to the behaviour of FeGeTe. [38, 39] Nevertheless, the overall magnetic ordering within FePdTe is FM, as the dominant magnitude of (32.8 meV) outweighs the weaker AF contribution from (-3.3 meV). In the studied range, we also include and couplings that encompass interchain interactions. The interactions between nearest interchain neighbours have values of = 0.1 and 0.06 meV as well as = 0.07 and 0.15 meV for FePdTe and CoPdTe, respectively, demonstrating the intrachain 1D nature of magnetic couplings. Interlayer couplings between adjacent layers were also computed, revealing an overall FM character in both materials. However, their magnitudes are considerably smaller compared to dominant intrachain interactions (Tables S1-4). The calculated for is 240K, which is not too far from the experimental value of 183K. On the other hand, is predicted to exhibit a lower of 140K, consistent with its weaker exchange interaction.

Figure 2. Top view of 1D chains of (a) FePdTe and (b) CoPdTe. For simplicity, we only depict the magnetic centres Fe and Co atoms. (c) Exchange interactions and for FePdTe (red) and CoPdTe (blue). (d) Orbital-resolved exchange coupling for FePdTe (left), CoPdTe (middle) and subtracted contribution, (right). (e) Same as (d), but for .
We further investigated the magnetic behaviour of upon partial atomic substitution, where 50% of the Fe atoms along each 1D chain are replaced by either Co or Ni, resulting in the compounds and , respectively. For such purpose, two different atomic configurations were examined. In the first one, referred as ALT, Fe atoms are substituted by Co (or Ni) in an alternating manner (Figure 3a,Figure 3b), with each Fe atom surrounded by two Co atoms. In the second arrangement, two consecutive Fe atoms are followed by two Co atoms, which we refer as CON. This results in each Fe atom being coordinated by one neighbouring Fe and one Co (Figure 3d,Figure 3e). Both structures were optimized, yielding similar lattice parameters, where the symmetry is retained (Table S5). A comparison between ALT and CON configurations reveals that the latter is energetically more favourable for both materials (Table S6). Regarding the magnetic properties, Table 1 summarizes the values of magnetic moments and MAE for these compounds. in the ALT configuration, the magnetic moments are 2.80 for Fe and 1.53 for Co, the latter enhanced relative to pristine (1.26 ) owing to the coordination with two neighbouring Fe atoms. In the CON configuration, magnetic moments of Fe and Co slightly decrease to 2.78 and 1.37 , respectively, as each Co atom is now coordinated with one Fe and one Co, exhibiting values closer to . For , Ni atoms exhibit minimal polarization, with magnetic moments of 0.23 (ALT) and 0.18 (CON), consistent with those reported for Ni-doped .[40] Regarding MAE, we observe a shift in the easy magnetic axis for in the ALT configuration from [101] to the [10] direction, with a corresponding MAE of -52.1 eV/magnetic atom, therefore stabilizing an out of plane magnetic ground state. This resembles the behaviour exhibited by Co-doped FeGeTe, where the addition of Co atoms modifies its magnetic easy axis.[31, 32] Conversely, in CON configuration, the system retains the magnetization along [101], requiring 0.16 meV to reorient spins towards either [101] or [10].
| Material | Arrangement | (Fe) | (Co) | (Ni) | [10] − [101] (meV/magnetic atom) | [10] − [101] (meV/magnetic atom) |
| FePdTe | — | 2.75 | — | — | 0.52 | 1.08 |
| FeCoPdTe | ALT | 2.80 | 1.53 | — | -0.052 | 0.047 |
| FeCoPdTe | CON | 2.78 | 1.37 | — | 0.16 | 0.16 |
| CoPdTe | — | — | 1.26 | — | 0.44 | 0.25 |
| FeNiPdTe | ALT | 2.80 | — | 0.23 | 0.77 | 0.64 |
| FeNiPdTe | CON | 2.78 | — | 0.18 | 0.49 | 0.21 |
Table 1. Values of and MAE for FePdTe, CoPdTe, FeCoPdTe and FeNiPdTe.
For FeNiPdTe, the magnetic easy axis remains unchanged. However, the MAE is lower in the CON configuration (0.49 meV/magnetic atom) compared to ALT (0.77 meV/magnetic atom), likely due to the presence of two consecutive non-magnetic Ni atoms per chain, which reduces the overall anisotropy.
We computed the magnetic exchange couplings and performed atomistic simulations to estimate the T. In the ALT configuration of FeCoPdTe, there is a strong FM coupling between Fe and Co atoms (18.8 meV). This is notably reduced compared to the Fe-Fe interaction in FePdTe (J = 32.8 meV), primarily due to the reduced magnetic moment of Co relative to Fe. Interactions between Fe-Fe and Co-Co retain their AF and FM characters, respectively, as in the pristine compounds. The estimated T for FeCoPdTe is 150K. A similar behaviour is observed in FeNiPdTe, where the FM coupling Fe-Ni is 5 meV. Furthermore, AF interaction between Fe atoms is significantly suppressed and the Ni-Ni coupling is negligible due to the minimal polarization of Ni atoms. As a result, the estimated is 100K, primarily driven by the Fe-Ni interaction.
According to our calculations, in the CON configuration for FeCoPdTe, there is a robust FM coupling of 27 meV between Fe and Fe sites along with more subtle FM couplings between Co-Fe and Co-Co. Unlike ALT, the CON configuration lacks short-range AF couplings between Fe-Fe. In contrast, its equivalent Fe-Co exchange is FM, showing a modest value of 1meV (Figure S5). Due to the enhanced FM character of the mentioned couplings and the suppression of competing AF interactions, the estimated increases from 150K in ALT to 170K in CON. For FeNiPdTe, the Fe-Fe FM coupling is 35 meV and the Ni-Fe interaction is 5 meV. However, the Ni-Ni coupling is effectively zero, consistent with the near-zero magnetic moment of Ni atoms. Although the overall ferromagnetism is enhanced compared to the ALT configuration, the system does not retain long-range magnetic ordering ( = 0K) due to the absence of short-range Ni-Ni interactions. Therefore, we foresee that the experimental incorporation of consecutive Ni atoms into the FePdTe lattice would suppress the net ferromagnetism along the 1D chains. Additionally, we computed the energy difference between interlayer AF and FM configurations for both compounds (Table S7). Our results indicate that the interlayer ferromagnetism is always retained, differently from the Co-induced antiferromagnetism observed in FeGeTe, FeGeTe and FeGaTe. [30, 31, 32, 33, 34]
Then, we examine the magnetic behaviour of FePdTe and CoPdTe under uniaxial strain along the intrachain [10] direction. The magnetic moments of Fe and Co atoms exhibit subtle variations under deformation (Figure S6). Regarding anisotropy, Figure 4a,Figure 4d indicate that the easy axis of magnetization is unaltered across the entire range, where MAE remains largely unaffected in FePdTe. By contrast, it increases under tensile strain in CoPdTe. From the evolution of magnetic couplings, one can observe that becomes more FM under compression, reaching 35.8 meV (-2%) for and 11.7 meV (-1.5%) for (Figure 4b,Figure 4e). Conversely, becomes more AF in due to an enhanced contribution from the - mechanism (Figure S7). Additionally, we computed the evolution of long-range exchange interactions, namely . These account for the sum of all the couplings beyond the nearest neighbours and . In both and , increases upon tensile strain. This, together with the observed trend of results in an enhancement of upon tensile strain and a decrease upon compression (Figure 4c,Figure 4f).

Figure 4. Evolution of (a) MAE, (b) exchange couplings , and and (c) for FePdTe upon applied strain along the [10] direction; and corresponding evolution of (d) MAE, (e) , and and (f) for CoPdTe.
The analysis of the magnon spectra for and reveals significant anisotropy (Figure 5) consistent with the previously discussed exchange interactions. In both compounds, strongly dispersive branches are observed along the direction, corresponding to magnons propagating along the 1D spin chains. In contrast, dispersion is notably weaker along directions perpendicular to them (e.g., or ), indicating suppressed interchain magnon transport. Under +2% tensile deformation, exhibits an ~8% reduction in the energy of optical magnons at , attributed to the strain-induced weakening of . Conversely, the energy of acoustic magnons increase with strain, reflecting the enhancement of . The same trend is observed for ; however, the optical magnons are marginally affected at due to the weaker strain dependence of in this compound.

Figure 5. Magnon dispersion for (a) FePdTe and (b) CoPdTe as a function of strain applied along the [10] direction.
In conclusion, we investigate the magnetic properties of using first principles calculations. Our results demonstrate that its magnetic behavior is predominantly governed by intrachain exchange interactions and , underscoring the 1D magnetic character of this 2D material. We also propose two new isostructural compounds, namely and , and confirm their dynamical stability. exhibits a FM ground state, while shows paramagnetic behavior. Furthermore, we provide a detailed microscopic analysis of the magnetic exchange interactions in and , revealing the distinct mechanisms underlying their magnetic behavior and show the potential of Co and Ni substitution to modulate the exchange couplings and anisotropy of . Finally, we demonstrate that mechanical strain offers an effective route for tuning the magnetic properties of and and show the pronounced anisotropy in their magnon spectra supports directional propagation of magnons along their 1D spin chains. Our findings highlight the potential of two-dimensional materials hosting 1D chains, and how their chemical and structural manipulation offers a promising platform for the design of magnetic and spintronic devices with tailored anisotropic characteristics.
Methods
DFT calculations on , and were performed using the VASP package[41] using the generalized gradient approximation (GGA). We relaxed both the atomic coordinates and lattice parameters employing a plane-wave cutoff of 400 eV. The Brillouin zone was sampled using a k-point Monkhorst–Pack that was increased to for the calculations of MAE. The phonon spectra for the three compounds were obtained using the Phonopy package[42] with supercells of dimensions . The magnetic couplings were evaluated as a function of distance until saturation using the TB2J software[43] and employing supercells of dimensions . A tight-binding Hamiltonian served as input for these calculations, obtained via the Wannier90 code,[44] with a reduced basis set formed by orbitals of Fe, Co and Ni as well as the orbitals of Pd and orbitals of Te. Simulations of were performed by means of the VAMPIRE code,[45] with 10000 steps for equilibration and averaging phases along with supercells of dimensions .
AUTHOR INFORMATION
Corresponding Author
*E-mail: [email protected].
Author Contributions
This work is part of the PhD thesis of A.M.R. All authors have given approval to the final version of the manuscript.
Notes
The authors declare no competing financial interest.
ACKNOWLEDGMENTS
The authors acknowledge the financial support from the European Union (ERC-2021-StG101042680 2D-SMARTiES) and the Excellence Unit “María de Maeztu” CEX2019-000919-M). J.J.B acknowledges the Generalitat Valenciana (grant CIDEXG/2023/1) and A.M.R. thanks the Spanish MIU (Grant No FPU21/04195). The calculations were performed on the Tirant III cluster of the Servei d’Informàtica of the University of València.
REFERENCES
Figures
References
- [1]Gibertini, M.; Koperski, M.; Morpurgo, A. F.; Novoselov, K. S. Magnetic 2D Materials and Heterostructures. Nat Nanotechnol 2019, 14 (5), 408–419.DOI
- [2]Wang, Q. H.; Bedoya-Pinto, A.; Blei, M.; Dismukes, A. H.; Hamo, A.; Jenkins, S.; Koperski, M.; Liu, Y.; Sun, Q.-C.; Telford, E. J.; Kim, H. H.; Augustin, M.; Vool, U.; Yin, J.-X.; Li, L. H.; Falin, A.; Dean, C. R.; Casanova, F.; Evans, R. F. L.; Chshiev, M.; Mishchenko, A.; Petrovic, C.; He, R.; Zhao, L.; Tsen, A. W.; Gerardot, B. D.; Brotons-Gisbert, M.; Guguchia, Z.; Roy, X.; Tongay, S.; Wang, Z.; Hasan, M. Z.; Wrachtrup, J.; Yacoby, A.; Fert, A.; Parkin, S.; Novoselov, K. S.; Dai, P.; Balicas, L.; Santos, E. J. G. The Magnetic Genome of Two-Dimensional van Der Waals Materials. ACS Nano 2022, 16 (5), 6960–7079.DOI
- [3]Li, H.; Ruan, S.; Zeng, Y. Intrinsic Van Der Waals Magnetic Materials from Bulk to the 2D Limit: New Frontiers of Spintronics. Advanced Materials 2019, 31 (27).DOI
- [4]Lee, K.; Dismukes, A. H.; Telford, E. J.; Wiscons, R. A.; Wang, J.; Xu, X.; Nuckolls, C.; Dean, C. R.; Roy, X.; Zhu, X. Magnetic Order and Symmetry in the 2D Semiconductor CrSBr. Nano Lett 2021, 21 (8), 3511–3517.DOI
- [5]Huang, B.; Clark, G.; Navarro-Moratalla, E.; Klein, D. R.; Cheng, R.; Seyler, K. L.; Zhong, D.; Schmidgall, E.; McGuire, M. A.; Cobden, D. H.; Yao, W.; Xiao, D.; Jarillo-Herrero, P.; Xu, X. Layer-Dependent Ferromagnetism in a van Der Waals Crystal down to the Monolayer Limit. Nature 2017, 546 (7657), 270–273.
- [6]Boix-Constant, C.; Mañas-Valero, S.; Ruiz, A. M.; Rybakov, A.; Konieczny, K. A.; Pillet, S.; Baldoví, J. J.; Coronado, E. Probing the Spin Dimensionality in Single-Layer CrSBr Van Der Waals Heterostructures by Magneto-Transport Measurements. Advanced Materials 2022, 34 (41).
- [7]Wang, X.; Du, K.; Fredrik Liu, Y. Y.; Hu, P.; Zhang, J.; Zhang, Q.; Owen, M. H. S.; Lu, X.; Gan, C. K.; Sengupta, P.; Kloc, C.; Xiong, Q. Raman Spectroscopy of Atomically Thin Two-Dimensional Magnetic Iron Phosphorus Trisulfide (FePS₃) Crystals. 2d Mater 2016, 3 (3), 031009.DOI
- [8]Deng, Y.; Yu, Y.; Song, Y.; Zhang, J.; Wang, N. Z.; Sun, Z.; Yi, Y.; Wu, Y. Z.; Wu, S.; Zhu, J.; Wang, J.; Chen, X. H.; Zhang, Y. Gate-Tunable Room-Temperature Ferromagnetism in Two-Dimensional Fe₃GeTe₂. Nature 2018, 563 (7729), 94–99.DOI
- [9]Fei, Z.; Huang, B.; Malinowski, P.; Wang, W.; Song, T.; Sanchez, J.; Yao, W.; Xiao, D.; Zhu, X.; May, A. F.; Wu, W.; Cobden, D. H.; Chu, J.-H.; Xu, X. Two-Dimensional Itinerant Ferromagnetism in Atomically Thin Fe₃GeTe₂. Nat Mater 2018, 17 (9), 778–782.DOI
- [10]May, A. F.; Ovchinnikov, D.; Zheng, Q.; Hermann, R.; Calder, S.; Huang, B.; Fei, Z.; Liu, Y.; Xu, X.; McGuire, M. A. Ferromagnetism Near Room Temperature in the Cleavable van Der Waals Crystal Fe₅GeTe₂. ACS Nano 2019, 13 (4), 4436–4442.DOI
- [11]Seo, J.; Kim, D. Y.; An, E. S.; Kim, K.; Kim, G.-Y.; Hwang, S.-Y.; Kim, D. W.; Jang, B. G.; Kim, H.; Eom, G.; Seo, S. Y.; Stania, R.; Muntwiler, M.; Lee, J.; Watanabe, K.; Taniguchi, T.; Jo, Y. J.; Lee, J.; Min, B. Il; Jo, M. H.; Yeom, H. W.; Choi, S.-Y.; Shim, J. H.; Kim, J. S. Nearly Room Temperature Ferromagnetism in a Magnetic Metal-Rich van Der Waals Metal. Sci Adv 2020, 6 (3).DOI
- [12]Zhang, G.; Guo, F.; Wu, H.; Wen, X.; Yang, L.; Jin, W.; Zhang, W.; Chang, H. Above-Room-Temperature Strong Intrinsic Ferromagnetism in 2D van Der Waals Fe₃GaTe₂ with Large Perpendicular Magnetic Anisotropy. Nat Commun 2022, 13 (1), 5067.DOI
- [13]Esteras, D. L.; Baldoví, J. J. Strain Engineering of Magnetic Exchange and Topological Magnons in Chromium Trihalides from First-Principles. Materials Today Electronics 2023, 6, 100072.DOI
- [14]Olsen, T. Magnetic Anisotropy and Exchange Interactions of Two-Dimensional FePS₃, NiPS₃ and MnPS₃ from First Principles Calculations. J Phys D Appl Phys 2021, 54 (31), 314001.
- [15]Shen, J.; Skomski, R.; Klaua, M.; Jenniches, H.; Manoharan, S. S.; Kirschner, J. Magnetism in One Dimension: Fe on Cu(111). Phys Rev B 1997, 56 (5), 2340–2343.DOI
- [16]Choi, D.-J.; Lorente, N.; Wiebe, J.; von Bergmann, K.; Otte, A. F.; Heinrich, A. J. Colloquium: Atomic Spin Chains on Surfaces. Rev Mod Phys 2019, 91 (4), 041001. https://doi.org/10.1103/RevModPhys.91.041001.
- [17]Nadj-Perge, S.; Drozdov, I. K.; Li, J.; Chen, H.; Jeon, S.; Seo, J.; MacDonald, A. H.; Bernevig, B. A.; Yazdani, A. Observation of Majorana Fermions in Ferromagnetic Atomic Chains on a Superconductor. Science (1979) 2014, 346 (6209), 602–607.
- [18]Li, S.; Wang, Y.; Hu, S.; Chen, D.; Zhang, C.; Yan, S. Robust Half-Metallicity in Transition Metal Tribromide Nanowires. Nanoscale 2018, 10 (33), 15545–15552.DOI
- [19]Lu, S.; Guo, D.; Cheng, Z.; Guo, Y.; Wang, C.; Deng, J.; Bai, Y.; Tian, C.; Zhou, L.; Shi, Y.; He, J.; Ji, W.; Zhang, C. Controllable Dimensionality Conversion between 1D and 2D CrCl₃ Magnetic Nanostructures. Nat Commun 2023, 14 (1), 2465.DOI
- [20]Lee, Y.; Choi, Y. W.; Lee, K.; Song, C.; Ercius, P.; Cohen, M. L.; Kim, K.; Zettl, A. 1D Magnetic MX₃ Single-Chains (M = Cr, V and X = Cl, Br, I). Advanced Materials 2023, 35 (49).DOI
- [21]Park, E.; Philbin, J. P.; Chi, H.; Sanchez, J. J.; Occhialini, C.; Varnavides, G.; Curtis, J. B.; Song, Z.; Klein, J.; Thomsen, J. D.; Han, M.; Foucher, A. C.; Mosina, K.; Kumawat, D.; Gonzalez-Yepez, N.; Zhu, Y.; Sofer, Z.; Comin, R.; Moodera, J. S.; Narang, P.; Ross, F. M. Anisotropic 2D van Der Waals Magnets Hosting 1D Spin Chains. Advanced Materials 2024, 36 (31).DOI
- [22]Lee, H.; Koo, C.; Choi, Y.; Oshima, Y.; Ulaganathan, R. K.; Kalaivanan, R.; Sankar, R.; Choi, K.-Y. Anomalous Spin Dynamics and Excitations of the Quasizigzag Chain Compound AgCrP₂S₆. Phys Rev B 2025, 111 (13), 134415.
- [23]Joy, P. A.; Vasudevan, S. Magnetism in the Layered Transition-Metal Thiophosphates MPS₃ (M =Mn, Fe, and Ni). Phys Rev B 1992, 46 (9), 5425–5433.pubmed.ncbi.nlm.nih.gov/10004324
- [24]Shi, B.; Geng, Y.; Wang, H.; Yang, J.; Shang, C.; Wang, M.; Mi, S.; Huang, J.; Pan, F.; Gui, X.; Wang, J.; Liu, J.; Xu, D.; Zhang, H.; Qin, J.; Wang, H.; Hao, L.; Tian, M.; Cheng, Z.; Zheng, G.; Cheng, P. FePd₂Te₂ : An Anisotropic Two-Dimensional Ferromagnet with One-Dimensional Fe Chains. J Am Chem Soc 2024, 146 (31), 21546–21554.DOI
- [25]Cenker, J.; Fonseca, J.; Nguyen, M.; Hu, C.; Chica, D. G.; Taniguchi, T.; Watanabe, K.; Zhu, X.; Roy, X.; Chu, J.-H.; Xu, X. Engineering Robust Strain Transmission in van Der Waals Heterostructure Devices. Nano Lett 2025, 25 (11), 4512–4517.DOI
- [26]Cenker, J.; Sivakumar, S.; Xie, K.; Miller, A.; Thijssen, P.; Liu, Z.; Dismukes, A.; Fonseca, J.; Anderson, E.; Zhu, X.; Roy, X.; Xiao, D.; Chu, J.-H.; Cao, T.; Xu, X. Reversible Strain-Induced Magnetic Phase Transition in a van Der Waals Magnet. Nat Nanotechnol 2022, 17 (3), 256–261.DOI
- [27]Silinskas, M.; Senz, S.; Gargiani, P.; Ruiz, A. M.; Kalkofen, B.; Kostanovski, I.; Mohseni, K.; Baldoví, J. J.; Meyerheim, H. L.; Parkin, S. S. P.; Bedoya-Pinto, A. Self-Intercalation as Origin of High-Temperature Ferromagnetism in Epitaxially Grown Fe₅GeTe₂ Thin Films. Phys Rev Lett 2024, 133 (25), 256702.DOI
- [28]Mak, K. F.; Shan, J.; Ralph, D. C. Probing and Controlling Magnetic States in 2D Layered Magnetic Materials. Nature Reviews Physics 2019, 1 (11), 646–661.DOI
- [29]Tian, C.-K.; Wang, C.; Ji, W.; Wang, J.-C.; Xia, T.-L.; Wang, L.; Liu, J.-J.; Zhang, H.-X.; Cheng, P. Domain Wall Pinning and Hard Magnetic Phase in Co-Doped Bulk Single Crystalline Fe₃GeTe₂. Phys Rev B 2019, 99 (18), 184428.DOI
- [30]Seo, J.; An, E. S.; Park, T.; Hwang, S.-Y.; Kim, G.-Y.; Song, K.; Noh, W.; Kim, J. Y.; Choi, G. S.; Choi, M.; Oh, E.; Watanabe, K.; Taniguchi, T.; Park, J.-H.; Jo, Y. J.; Yeom, H. W.; Choi, S.-Y.; Shim, J. H.; Kim, J. S. Tunable High-Temperature Itinerant Antiferromagnetism in a van Der Waals Magnet. Nat Commun 2021, 12 (1), 2844.DOI
- [31]Tian, C.; Pan, F.; Xu, S.; Ai, K.; Xia, T.; Cheng, P. Tunable Magnetic Properties in van Der Waals Crystals (Fe₁₋ₓCoₓ)₅GeTe₂. Appl Phys Lett 2020, 116 (20).DOI
- [32]May, A. F.; Du, M.-H.; Cooper, V. R.; McGuire, M. A. Tuning Magnetic Order in the van Der Waals Metal Fe₅GeTe₂ by Cobalt Substitution. Phys Rev Mater 2020, 4 (7), 074008.DOI
- [33]Zhu, K.; Wang, M.; Deng, Y.; Tian, M.; Lei, B.; Chen, X. Effect of Co or Ni Substitution on Magnetism in the Layered van Der Waals Ferromagnet Fe₃GaTe₂. Phys Rev B 2024, 109 (10), 104402.
- [34]Wang, M.; Zhu, K.; Lei, B.; Deng, Y.; Hu, T.; Song, D.; Du, H.; Tian, M.; Xiang, Z.; Wu, T.; Chen, X. Layer-Number-Dependent Magnetism in the Co-Doped van Der Waals Ferromagnet Fe₃GaTe₂. Nano Lett 2024, 24 (14), 4141–4149.DOI
- [35]Qiao, L.; Li, M.; Cui, Y.; Xu, S.; Reimers, J. R.; Ren, W. Giant Carrier Mobility in a Room-Temperature Ferromagnetic VSi₂N₄ Monolayer. Nano Lett 2024, 24 (21), 6403–6409.DOI
- [36]Deiseroth, H.; Aleksandrov, K.; Reiner, C.; Kienle, L.; Kremer, R. K. Fe₃GeTe₂ and Ni₃GeTe₂ – Two New Layered Transition-Metal Compounds: Crystal Structures, HRTEM Investigations, and Magnetic and Electrical Properties. Eur J Inorg Chem 2006, 2006 (8), 1561–1567.
- [37]Chen, X.; Shao, Y.-T.; Chen, R.; Susarla, S.; Hogan, T.; He, Y.; Zhang, H.; Wang, S.; Yao, J.; Ercius, P.; Muller, D. A.; Ramesh, R.; Birgeneau, R. J. Pervasive beyond Room-Temperature Ferromagnetism in a Doped van Der Waals Magnet. Phys Rev Lett 2022, 128 (21), 217203.DOI
- [38]Ruiz, A. M.; Esteras, D. L.; López-Alcalá, D.; Baldoví, J. J. On the Origin of the Above-Room-Temperature Magnetism in the 2D van Der Waals Ferromagnet Fe₃GaTe₂. Nano Lett 2024, 24 (26), 7886–7894.DOI
- [39]Shen, Z.-X.; Bo, X.; Cao, K.; Wan, X.; He, L. Magnetic Ground State and Electron-Doping Tuning of Curie Temperature in Fe₃GeTe₂ : First-Principles Studies. Phys Rev B 2021, 103 (8), 085102.DOI
- [40]Ghosh, S.; Ershad, S.; Sanyal, B. Structural Distortion and Dynamical Electron Correlation Driven Enhanced Ferromagnetism in Ni-Doped Two-Dimensional Fe₅GeTe₂ beyond Room Temperature. 2d Mater 2024, 11 (3), 035002.DOI
- [41]Kresse, G.; Furthmüller, J. Efficient Iterative Schemes for Ab Initio Total-Energy Calculations Using a Plane-Wave Basis Set. Phys Rev B 1996, 54 (16), 11169–11186.pubmed.ncbi.nlm.nih.gov/9984901
- [42]Togo, A.; Tanaka, I. First Principles Phonon Calculations in Materials Science. Scr Mater 2015, 108, 1–5.arxiv.org/abs/1506.08498
- [43]He, X.; Helbig, N.; Verstraete, M. J.; Bousquet, E. TB2J: A Python Package for Computing Magnetic Interaction Parameters. Comput Phys Commun 2021, 264, 107938.
- [44]Mostofi, A. A.; Yates, J. R.; Lee, Y.-S.; Souza, I.; Vanderbilt, D.; Marzari, N. Wannier90: A Tool for Obtaining Maximally-Localised Wannier Functions. Comput Phys Commun 2008, 178 (9), 685–699.DOI
- [45]Evans, R. F. L.; Fan, W. J.; Chureemart, P.; Ostler, T. A.; Ellis, M. O. A.; Chantrell, R. W. Atomistic Spin Model Simulations of Magnetic Nanomaterials. Journal of Physics: Condensed Matter 2014, 26 (10), 103202.DOI