betaFeedback

WorksPhysics and Astronomy

The impact of hydrostatic pressure, nonstoichiometry, and doping on trimeron lattice excitations in magnetite during axis switching

Abstract

Trimeron lattice excitations in single crystalline magnetite, in the form of the cc axis switching (i.e. the reorganization of the lattice caused by external magnetic field) at temperatures below the Verwey temperature TVT_V are observed by magnetization experiments. These excitations exhibit strong sensitivity to doping (with Zn, Al, and Ti), nonstoichiometry and hydrostatic pressure (p<1.2p < 1.2 GPa). The considered indicators of the axis switching (AS) are: the switching field BswB_{sw}, the energy density needed to switch the axis EswE_{sw} and the activation energy UU. Our results show that hydrostatic pressure pp weakens the low−T-T magnetite structure (decreases TVT_V) and has roughly similar effects on AS in Zn-doped Fe3_3O4_4 and, in much less extent, in stoichiometric magnetite. We have, however, found that while doping/nonstoichiometry also lowers TVT_V, making it more prone to temperature chaos, it drastically increases the switching field, activation and switching energies suggesting that the trimeron order, subject to change while AS occurs, is more robust. Consequently, we conclude that the manipulation of trimerons in the process of axis switching and the mechanisms leading to the Verwey transition are distinct phenomena.

Introduction

The charge and orbital order in magnetite at T<TVT < T_{\mathrm{V}}, where TVT_{\mathrm{V}} is the Verwey temperature, exhibits characteristic cigarlike structures in a form of polarons known as trimerons [1]. Recently, spectroscopic signatures of the low-energy electronic excitations of the trimeron network were reported [2]. In seemingly unrelated experiments, we have been observing the magnetic field-induced manipulation of the monoclinic cc axis in the process referred to as “axis switching” (AS). Since AS also impacts the trimeron order, this phenomenon represents an alternative method to excite the trimerons. In this study, we present the investigation of these excitations under various conditions, including sample defect structure (nonstoichiometry, Zn, Al, and Ti doping) and hydrostatic pressure up to 1.2 GPa. These investigations were performed using magnetic moment vs. applied magnetic field, m(B)m(B), measurements.

Magnetic axis switching in magnetite was first mentioned and analysed by Calhoun in 1954 [3] in his magnetization vs. magnetic field experiments, but the phenomenon was also observed in other materials [4, 5, 6]. Below the isotropy point of TIP=130T_{\mathrm{IP}} = 130 K (where anisotropy energy in magnetite is minimal) the easy magnetization axis is in one of <100> directions (see e.g. [7]) and this is preserved when cooling magnetite below TVT_{\mathrm{V}} at which point cubic symmetry turns to monoclinic: each cubic <100> may become the monoclinic cc axis and, simultaneously, the easy magnetic axis. Therefore, the material breaks into structural domains on cooling [three of them, with different cc axes, are shown symbolically in Figure 1a1 [8, 9]. An external magnetic field B>0.2B > 0.2 T applied along one of the ⟨001⟩\langle001\rangle crystallographic axes during cooling across TVT_{\mathrm{V}} may force the magnetic easy axis along this particular direction [8] Figure 1b, what is proved by the characteristic m(B)m(B) relation Figure 1c. If the sample is now magnetized along the other ⟨100⟩\langle100\rangle direction below TVT_{\mathrm{V}} (and at TT higher than 50 K), a reorientation of magnetic moments, i.e., axis switching, takes place and this ⟨100⟩\langle100\rangle direction becomes a new easy axis [3, 8, 9, 10].

Image not extracted

Figure 1. Cooling a magnetite sample below TVT_{\mathrm{V}} results either with three principle domains of monoclinic CcCc structure with cc easy axes along previous cube edges (a), or one cc axis (b) when the external magnetic field along one of the cube edges is applied on cooling. Subsequent field application (at T>50T > 50 K) along one of the two other cube directions initially has no effect, but eventually can switch irreversibly the axis that can best be observed in mm vs BB experiment (c); here the dashed arrows indicate the change of magnetic field, while the bold arrow points to the switching field BswB_{\mathrm{sw}}. The shaded area in the plot in panel (c) is a measure of energy needed to switch the axis, i.e. is proportional to the switching energy density EswE_{\mathrm{sw}}. The figure is a part of mm vs BB measurement for sample #1 (the complete data are presented in Figure 3Sa in Supplemental Material (SM) [11].

Calhoun [3] showed that the magnetic field BswB_{\mathrm{sw}} needed to switch the axis depends on temperature TT, activation energy UU, and is observed when the process starts to have a collective behavior (this is depicted by the CC parameter; only above some threshold CC value, the process starts to be experimentally observed). It all resulted in the characteristic formula Bswi=CTexp⁡(U/kBT)B_{\mathrm{sw}}^{i}=CT\exp(U/k_{\mathrm{B}}T) (BswiB_{\mathrm{sw}}^{i} in the internal switching field) that links all the parameters mentioned above.

Subsequent studies have revealed that not only the magnetic axes but also the crystal axes, and thus the trimeron lattice, undergo irreversible changes in response to the external magnetic field. We have extensively explored this phenomenon using various experimental techniques, including global probes such as magnetization [8], symmetry oriented techniques such as x-ray diffraction (XRD) [9] and resonant x-ray scattering (RXS) [12], as well as microscopic methods such as nuclear magnetic resonance (NMR) [13] and Mössbauer spectroscopy (MS) [12]. In essence, these experiments demonstrated that each manipulation of the cc axis is an excitation of the trimeron lattice.

It is worth noting that the trimeron lattice is not only a structural building block but also a fundamental element of magnetite’s electronic structure. As recently demonstrated, the trimeron lattice critically softens at TVT_{\mathrm{V}}, indicating its intimate link with the Verwey transition [2]. Furthermore, the transition is highly sensitive to even minor perturbations of the lattice, such as doping and nonstoichiometry. For instance, already 1/3% of Fe ions are already either vacant or replaced with Zn, and Ti lowers TVT_{\mathrm{V}} by 15 K. Higher doping changes the character of the transition (refer to Sec. I in [11]), and 1% suppresses the transition entirely. Hydrostatic pressure also exerts a significant influence on the transition by reducing TVT_{\mathrm{V}}.

Hence, the observation of AS, which represents an alternative means of modifying the trimeron system, and investigating how this process depends on sample doping and pressure can provide valuable insights into the understanding of the switching mechanism itself. Moreover, these investigations can contribute to a better understanding of the trimeron structure, trimeron excitation spectrum and, ultimately, the Verwey transition (VT). It can, also, help to describe possible trimeron order that exists, in some extent, above TVT_{\mathrm{V}}, where it is dynamic rather than static [14], or its potential role in creating electronic nematic order characterized by static, low-value electronic disproportionation, as recently proposed [15].

This study primarily focuses on the excitations of the trimeron lattice and the mechanism underlying the AS. We explore how AS, represented by changes in the m(B)m(B) behavior, responds to various kinds of defects (nonstoichiometry, Zn, Al, and Ti doping), or hydrostatic pressure. We have deliberately selected nonmagnetic dopants to avoid introducing additional variables; however, these dopants possess distinct valences and locate at different lattice positions. Finally, the defect concentration (dopants and Fe vacancies) was high enough to considerably alter TVT_{\mathrm{V}} while maintaining the discontinuous character of the VT. Low hydrostatic pressure also affects TVT_{\mathrm{V}} by inducing changes in the electronic, rather than the defect structure, thus providing insights into the electronic aspects of AS. Additionally, we have investigated the response of the trimeron order to the sequential manipulation of the sample structure, referred to as "sample training"; this is shown in [11].

We investigated several key parameters that provide quantitative characterization of the AS process. These parameters include the switching field BswB_{\mathrm{sw}} and switching energy density EswE_{\mathrm{sw}} [see Fig. 1c], both directly derived from the mm vs BB experiments, as well as the fitting parameter UU, which represents the activation energy. We have discovered that through increasing the temperature, increasing number of structural twins (caused by sample training, see Sec. 4(d) in [11]), or by applying hydrostatic pressure, the trimeron lattice becomes more susceptible to changes, reflected in decreasing the switching field BswB_{\mathrm{sw}} and switching energy EswE_{\mathrm{sw}}. On the contrary, doping or nonstoichiometry appear to strengthen the trimeron order increasing BswB_{\mathrm{sw}} and EswE_{\mathrm{sw}}. Furthermore, the activation energy UU exhibits an increase with doping or nonstoichiometry, while the impact of pressure on UU differs between doped and stoichiometric magnetite. Specifically, UU appears to be pressure independent for stoichiometric magnetite, whereas it decreases under pressure for Zn-doped sample.

The structure of the paper is as follows: In Sec. 2, we present the characterization of the sample and the experimental procedures. This is followed by the presentation of results of AS in different scenarios, including stoichiometric and nonstoichiometric magnetite as well as Zn-, Al-, and Ti-doped samples, and finally studies conducted under hydrostatic pressure (Sec. 3). Our findings are discussed in Sec. 4 and the article is concluded in § 11.

Samples and experimental procedure

Single crystals of stoichiometric, nonstoichiometric, and doped magnetite were grown from the melt by the cold crucible technique (skull melter) at Purdue University, USA [16]. The crystals were subsequently annealed to achieve the appropriate metal to oxygen ratio [17, 18]. The samples included magnetite with varying levels of nonstoichiometry, 3δ3\delta in Fe3(1−δ)O4\mathrm{Fe}_{3(1-\delta)}\mathrm{O}_{4} with values of 3δ=03\delta= 0, 0.0075 and 0.0105. In addition, doping was performed with zinc, Fe3−xZnxO4\mathrm{Fe}_{3-x}\mathrm{Zn}_{x}\mathrm{O}_{4}, (x=0.0066x = 0.0066, x=0.007x = 0.007 and x=0.01x = 0.01), aluminum, Fe3−xAlxO4\mathrm{Fe}_{3-x}\mathrm{Al}_{x}\mathrm{O}_{4}, (x=0.012x = 0.012), and titanium Fe3−xTixO4\mathrm{Fe}_{3-x}\mathrm{Ti}_{x}\mathrm{O}_{4}, (x=0.01x = 0.01). It is important to note that the chosen doping levels and nonstoichiometry were deliberately kept small to only subtly alter the properties of magnetite and maintain a discontinuous character of the Verwey transition (x=3δ≤0.012x = 3\delta\le0.012). The effects of doping and nonstoichiometry on A (tetrahedral) and B (octahedral) sites in magnetite structure, as well as their impact on the Verwey transition in general, are elaborated in Sec. 1 of [11] and Refs. [18, 19, 20, 21, 22, 23] therein. To assess the quality of the samples, the width of the Verwey transition in the temperature dependence of ac susceptibility was examined. The results of these tests, along with the respective values of TVT_{\mathrm{V}}, along with selected details of the samples, are presented in the Table 1, and furthermore illustrated graphically in Figure 1S of [11].

All measurements described below were performed using Vibrating Sample Magnetometer [(VSM); Princeton Applied Research, PAR Model 4500 with cryostat Model 153 and Varian 12-in. electromagnet, controlled by the Lakeshore VSM Controller 7300]. In the case of the experiments conducted under pressure (up to 1.2 GPa), the description of the cell and the setup can be found in Ref. [24], with some details presented in [11] (Figure 3S).

Image not extracted

Figure 3. Temperature dependence of the energy density EswE_{\mathrm{sw}} (in Kelvin per one Fe atom) required to switch the axis. Representative error bars are shown for two cases (sample Zn #3, p=0.64p = 0.64 and 1.131.13 GPa). The data for separate cases: for samples under ambient pressure and pressure dependence for #3 and Zn #3 are given in Figure 7S(b) and 12S(b), respectively.

SampleTVT_{\mathrm{V}} (K)U/kBU/k_{\mathrm{B}} (K)Uncertainty of UU Δ(U/kB)\Delta(U/k_{\mathrm{B}}) (K)
Fe3_3O4_4 #1 (cylinder)123.735814
Fe3_3O4_4 #2 (sphere)123.847023
Fe3_3O4_4 #3 (cylinder) used for pressure studies12433711
Fe3(1−δ)_{3(1-\delta)}O4_4, 3δ=0.00753\delta= 0.0075114.874760
Fe3(1−δ)_{3(1-\delta)}O4_4, 3δ=0.01053\delta= 0.0105109.784635
Fe3−x_{3-x}Znx_xO4_4. Zn #1 (xZn=0.007x_{\mathrm{Zn}} = 0.007)114.458410
Fe3−x_{3-x}Znx_xO4_4. Zn #2 (xZn=0.01x_{\mathrm{Zn}} = 0.01)110.868854
Fe3−x_{3-x} Znx_xO4_4. Zn #3(xZn=0.0066x_{\mathrm{Zn}} = 0.0066) used for pressure studies114.549020
Fe3−x_{3-x}Alx_xO4_4, xAl=0.012x_{\mathrm{Al}} = 0.012112.868250
Fe3−x_{3-x}Tix_xO4_4, xTi=0.01x_{\mathrm{Ti}} = 0.01111.4900200

Table I. Results of the samples characterization (TVT_{\mathrm{V}}; Zn, Al, Ti concentration and δ\delta) and fitted parameter UU describing temperature dependence of the switching field. Zn and Ti concentration xx were drawn from TVT_{\mathrm{V}} vs xx relation (Figure 1S(b) in SM), Al content was measured by x-ray microprobe, and δ\delta was set by the annealing conditions.

In all magnetization experiments (one sphere and nine cylinders of various radius), the cylinder axis (and one of the <100><100> axes in the case of a sphere) was set along the VSM vertical probe (note that cubic notation will be used throughout the rest of the paper). Two other <100><100> directions in the horizontal plane were identified at 290 K in 0.15–0.3 T field as these directions with the smallest moment (since these directions were hard axes in the high TT phase of magnetite), see Figure 4S(b) and 4S(f) in SM [11]. After horizontal <100><100> axes were found, the samples were cooled to the specified temperature below TVT_{\mathrm{V}} in magnetic field larger than 0.5 T (which was proved to be strong enough to define the cc axis [8]; see Sec. 2 and Figure 2S in SM [11] for further discussion) set along the [100] direction (as schematically shown in Figure 1). This field-cooling (FC) procedure establishes an easy axis in this particular direction, what is confirmed by the m(B)m(B) measurement with BB along this direction (Figure 1c, blue line).

Image not extracted

Figure 2. Temperature dependence of the switching field, Bi_swB_{\mathrm{i\_sw}} for all studied samples. The data for separate cases: for samples under ambient pressure and pressure dependence for #3 and Zn #3 are also presented in [11] [Figure 7S(a) and 12S(a), respectively].

Image not extracted

Figure 4. Correlation between activation energy UU and the Verwey transition temperature TVT_{\mathrm{V}}.

The subsequent steps were as follows:

  • The mm vs. BB measurements were typically conducted at a specified temperature with a magnetic field applied along the initially defined easy axis [this is the blue line in Figure 1(c)]. From the initial part of the m(B)m(B) curve, the demagnetization factor DD was calculated, which was used later to determine the internal field Bi_swB_{i\_sw}; in this linear region of the m(B)m(B) curve the external field compensates the demagnetizing field.

  • The sample was then rotated by 90° to align the magnetic field along the other ⟨100⟩\langle100\rangle direction, referred to as [10], an unspecified magnetic direction below TVT_{\mathrm{V}}. The resulting m(B)m(B) curve obtained at 4.2 K is presented as the red line in Figure 1(c).

  • At sufficiently high temperature, the axis switching occurred, eventually setting the new easy axis direction along the applied magnetic field, represented by orange dots in Figure 1(c).

  • The sample was subsequently heated above TVT_{\mathrm{V}} and again field cooled along the [100] direction to a new temperature below TVT_{\mathrm{V}}. At this temperature, measurements of m(B)m(B) along [100] and along [10] were repeated.

Experimental results

Ambient pressure data

The switching field BswB_{\mathrm{sw}}, which is the most direct experimental parameter extracted from our measurements, was determined from each of the m(B)m(B) curves acquired along the magnetically unspecified axes. The recalculation of BswB_{\mathrm{sw}} into the intrinsic field Bi_swB_{\mathrm{i\_sw}} was performed using the demagnetization parameters DD, see Figure 1. Bi_swB_{\mathrm{i\_sw}} vs TT plots for all the studied samples, including those under elevated pressure, are shown in Figure 2. Although cumulative figures, like this one, best present the clear tendency of the parameters drawn from the measurements performed on all of the samples, for clarity, Bi_swB_{\mathrm{i\_sw}} vs TT is further plotted separately for samples under ambient pressure, and the pressure dependence of Bi_swB_{\mathrm{i\_sw}} in Figure 7S(a) and Fig. 12S(a) of [11], respectively.

Image not extracted

Figure 7. m(B)m(B) under p=1.2p = 1.2 GPa at different temperatures. The data at 10 K prove that the cc and magnetic easy axes are well defined: dashed blue line is along an easy direction [100], while blue solid line is along an unspecified direction [10]. At 100 K the situation is different: m(B)m(B) along the “easy” [100] shows a reversible hysteresis (black line), repeatable (red line). m(B)m(B) along “unspecified” [10] (green) also shows hysteresis, but irreversible. Note that m(B)m(B) on BB lowering is more steep along [10] (i.e. after “axis switching”) than along the easy axis [100].

All the data were extracted from the results of magnetic moment vs magnetic field measurements performed at several temperatures for three stoichiometric, two nonstoichiometric, as well as in three Zn-doped, one Al-doped, and one Ti-doped samples, under ambient and increased pressure; the results are presented in Figure 4S, Figure 5S, Figure 6S, 9S and 11S in [11] and in Figure 5 below.

Image not extracted

Figure 5. Representative results of pressure (a) measurements of the stoichiometric sample Fe3O4\mathrm{Fe}_3\mathrm{O}_4 #3 (m(B)m(B) for ambient pressure is in Figure 4S(d) in [11]). In panels (b), (c) ln⁡(Bsw/T)\ln(B_{\mathrm{sw}}/T) vs 1000/T1000/T and the ensuing UU values for all pressure values are presented for Fe3O4\mathrm{Fe}_3\mathrm{O}_4 #3 and Zn-doped magnetite, respectively. See SM [11] for the collection of all data and more discussions of the results for 1.2 GPa in Fe3O4\mathrm{Fe}_3\mathrm{O}_4 #3.

Image not extracted

Figure 6. (a) Pressure dependence of Bi,swB_{i,\mathrm{sw}} at two representative temperatures for stoichiometric (Fe3_3O4_4 #3) and Zn doped magnetite (Fe3−x_{3-x}Znx_xO4_4 Zn #3). The plots are cuts along the dotted lines in Figure 2. Panel (b) presents the pressure dependence of UU measured in the same samples.

In Figure 3, we illustrate the energy (work), EswE_{\mathrm{sw}}, needed to switch the easy cc axis, estimated from the m(B)m(B) curves [see Figure 1(c) for EswE_{\mathrm{sw}} definition]. The temperature dependence of Bi,swB_{\mathrm{i,sw}}, represented as ln⁡(Bi,sw/T)\ln(B_{\mathrm{i,sw}}/T) vs 1000/T1000/T, was fitted with Calhoun’s formula Bi,sw=CTexp⁡(U/kBT)B_{\mathrm{i,sw}} = CT\exp(U/k_{\mathrm{B}}T). The activation energy UU, one of the fitting parameters which is the second important value characterizing AS, is shown in Figure 4 as a function of TVT_{\mathrm{V}}. The fits are presented in Figure 4S, Figure 5S, Figure 6S, 9S, 11S in [11] and in Figure 5.

Experiments at elevated pressure

Two samples, one stoichiometric magnetite, Fe3_3O4_4 #3, and one Zn doped (Fe3−x_{3-x}Znx_xO4_4 Zn #3, see Figure 6S(c), and 6S(h) in [11], where the ambient pressure results for this sample are shown), were measured under elevated pressure. After the <100><100> directions perpendicular to the cylinder axis were found (which was done at 160160 K to let the transmitting pressure oil to freeze), a sample was field-cooled (FC) down to the lowest temperature (below 2020 K). Representative results of m(B)m(B) for stoichiometric sample #3 and under p=0.75p = 0.75 GPa are shown in Figure 5(a) (complete results are provided in Figs. 9S and 11S in [11]).

As before, UU was estimated from ln⁡(Bi,sw/T)\ln(B_{\mathrm{i,sw}}/T) vs. 1000/T1000/T curves, shown in Figure 5(b) (stoichiometric sample) and in Figure 5(c) (Zn doped).

The procedure of setting the easy direction along the cooling field proved to be effective in the case of the pressure p=1.2p = 1.2 GPa for undoped sample x=0x = 0 at temperatures below 65 K. However, at higher temperatures, above ca. 70 K, m(B)m(B) along [100] (expected to be an easy axis after FC) did not exhibit typical behavior of an easy axis. This phenomenon will be further discussed in Sec. 4 c below.

Additionally, the results pertaining to the pressure dependence of the magnetic moment step at TVT_{\mathrm{V}} (aimed to determine the Verwey transition temperature vs pp) and pressure dependence of magnetic moment are presented in Figs. 13S and 14S in [11], where our data are further discussed in the context of the results published in Refs. [25, 26, 27, 28, 29, 30] [31] therein.

Discussion

An effort was already made to observe AS more microscopically, by NMR [13] or Mössbauer spectroscopy [12], to see the individual Fe positions that either change during AS, as BB positions, or observe the ongoing process without changing their valence (as AA positions). With all these efforts in mind, our aim here was to observe the AS process from a more global perspective, although based on quantitative parameters, BswB_{\mathrm{sw}}, energy EswE_{\mathrm{sw}}, and the activation energy UU.

Before delving into the discussion, it is important to clarify that there are multiple trimeron excitations present. Each absorption of energy by magnetite corresponds to a reconfiguration of electronic states, i.e. some trimeron excitation. Among these excitations, the one which appears to be most intimately linked to AS is magnetocrystalline energy. When a magnetic field is applied, magnetic moments, or electronic orbitals tied to the spins via, mainly, spin-orbit coupling (SOC), are affected. Initially, the domain wall movement takes place, indicating that individual spins in trimerons incline towards the field direction (i.e. some elementary excitation takes place). Once completed, the volume magnetic moment partly rotates towards the field direction, causing the excitation of the trimerons from their normal state. It is important to note that such processes are not considered in our studies, although their relation to magnetic anisotropy is discussed further below in Sec. 4 d. Our focus solely revolves around crystallographic structure changes triggered by the magnetic field. It should be noted that there are additional structure-related excitations as mentioned in Ref. [32]. These include the appearance of aa- and bb-axis structural domains spontaneously appearing just below TVT_{\mathrm{V}}, possibly related to additional cc-axis twins (although not observed in Ref. [32]). Such considerations appear to be a natural extension of the phenomena we present here.

The main results of our study are presented in Figure 2-Figure 4, with additional results for elevated pressure provided in SM [11].

Several noteworthy findings include the following:

Temperature dependence of AS process

When the temperature is increased, BswB_{\mathrm{sw}} and AS energy EswE_{\mathrm{sw}}, which is closely related to BswB_{\mathrm{sw}} decrease. In each system, as TT increases, the occupation probability of higher-energy states also increases resulting in changes across the entire system. In the case a phase transformation, like the Verwey transition, is approached, not only do the energy levels become more populated, but this increased population also alters the states themselves, causing their energy to decrease. Consequently, their population continues to rise, ultimately leading to critical fluctuations and a phase transition. Each subsystem of the whole entity changes this way: it was shown, e.g., for trimeron elementary excitations [2] where the energy level separation of 5 meV decreased almost to zero just below TVT_{\mathrm{V}}. The natural question arises: Is there any specific subsystem whose behavior dominates and acts as a leading force of the transition, shaping the temperature dependence of other subsystems?

Several phenomena can be considered here, such as the dependence of the spin-orbit coupling on TT [33] and lattice vibrations [35,36]. However, as the more detailed discussion in SM [11] elucidates, these factors appear to be unlikely contributors. Nevertheless, there is a 25% decrease in the electric field gradient with increasing TT for C3 and C4, representing two of the four components of the stoichiometric magnetite Mössbauer spectrum (see Figure 3 in [34]). If the atoms constituting these components are actively involved in AS, as discussed further in Secs. 4 b and 4 d, and also in SM [11], our observation could potentially provide an explanation for the pronounced TT dependence of the AS.

The work required to switch the axis, EswE_{\mathrm{sw}}, is strictly linked to BswB_{\mathrm{sw}} and is also TT dependent. Although it is a value associated with the collective process, i.e. an excitation of all trimerons simultaneously, the small value of the energy (0.25 K per Fe atom at lowest accessible temperatures down to 0.05 K at highest, close to TVT_{\mathrm{V}}) is approximately 100 times lower than 5 meV reported in [2] also for some collective process engaging trimerons. This contrast implies that when employing a magnetic field, we are probing a distinct trimeron excitation compared to the one documented in [2]. In the latter case, the observed process involved the sliding of trimerons, whereas in our study, we observe their rotation as the dominant mode of excitation.

Dopant and nonstoichiometry dependence

Doping and nonstoichiometry, each accounting for less than 1/3% of the total iron content, considerably increase BswB_{\mathrm{sw}}, AS energy EswE_{\mathrm{sw}}, and UU. Consequently, a greater effort is needed to reorganize the trimerons. This effect, vividly presented in Figure 2-Figure 4, represents the most significant result of our studies and surpasses any potential parameter changes arising from the inevitable slight variations among the three nominally identical stoichiometric samples. This is equally strong, but opposite effect to TVT_{\mathrm{V}} vs. xx dependence, where also small amounts of defects considerably affect the transition, even changing its character (see Figure 4 where the anticorrelation of UU with TVT_{\mathrm{V}} is presented. For the discussion of defects occupancy see Sec. 1 in SM [11]). This anticorrelation would suggest that "more rigid" trimerons make the Fe-B lattice more vulnerable to temperature disorder (lower TVT_{\mathrm{V}}). This idea is not easy to accept bearing in mind that electrons within trimerons, and their confinement to the lattice (strong electron-phonon interactions) are usually reported in literature as being strictly connected with the mechanism of the Verwey transition.

However, it was shown in [37,38], the change of lattice distortion precedes the change of orbital and charge ordering on heating, as if electron ordering (charge in trimerons) sluggishly adjusted to already altered lattice. In case of further decrease of electron-lattice interactions, i.e. a possible effect of doping, electron charge may be changed by magnetic field with the lattice being inactive. This means that the easy axis does not change, i.e. there is no visible AS, despite some electronic rearrangement within trimerons. This idea is, however, not further supported by experiment because stoichiometric and slightly Zn-doped magnetite crystals show the same difference in lattice distortion and charge/orbital ordering temperatures, [37,38] yet their response to magnetic field, AS, is drastically different. Also, no clear change in electronic states is visible in slightly doped magnetite (as studied here) unlike in magnetite exhibiting continuous VT [39]. Therefore, we consider the above model as speculative, and the ultimate suggestion is that what we observe as the reorganization of electronic order (seen by us as a trimeron rearrangement) is not the same electronic reorganization as the one that takes place at TVT_{\mathrm{V}}. This is additionally supported by the fact that TVT_{\mathrm{V}} lowers with the increase of the content of Zn, Ti, and 3δ3\delta in another way than with the content of Al (see Figure 1S(a) in SM [11]), while the results for UU, BswB_{\mathrm{sw}} and EswE_{\mathrm{sw}} dependence on xx and δ\delta are all very similar.

Doped magnetite was studied microscopically by NMR [40] and MS [34]. Although only a minor change of resonance field was observed in low Zn- and Ti-doped magnetite (with discontinuous VT) in NMR results, the rapid change of hyperfine magnetic field on Fe sites is visible once xx enters the second order Verwey transition regime, very close to the concentration we study here. This roughly coincides with the remark in [41] about highly selective oxidation of one particular BB position on Zn doping or nonstoichiometry, in about the same xx region where first order magnetite turns to second order. Note, however, that the effect of doping is element selective [40] even if the same Fe position is replaced, unlike in TVT_{\mathrm{V}} vs xx (for Zn, Ti, and 3δ3\delta) and as in our case of AS. However, the drop of the hyperfine field is universal.

The same conclusion of the drastic change of the system properties on doping when entering the second order regime is visible in MS results [34]: with increasing the temperature (below TVT_{\mathrm{V}}), there is a substantial drop of the electric field gradient VzzV_{zz} in eight Fe octahedral positions (belonging to the C3 and C4 components mentioned above) with even a change of sign in one of those (C3). This is in accord with the increased value of activation energy UU in doped/nonstoichiometric samples that shows the pace of BswB_{\mathrm{sw}} changes with TT (the higher UU, the more dependent on TT the switching field BswB_{\mathrm{sw}} is). The arguments for C3 and C4 involvement in AS are further shown in Sec. 4 d below.

No matter how subtle the electronic changes caused by doping/nonstoichiometry in seven measured samples might be, BswB_{\mathrm{sw}} behaves as if trimerons were pinned by defects caused by dopants/nonstoichiometry. Thus our results also show that any general claims drawn from nonideal crystals and concerning electronic trimeron structure can be questioned (see, e.g., [15]). The same phenomenon, of defects impact on material properties, is present in superconductors where defects pin vortices which makes current flow nondissipative.

The important role the defects (of several kinds) play in magnetite microstructure and the ensuing properties was already commented on, e.g., in [42], where the step in ac susceptibility was suggested to be due to magnetic domain walls pinning on crystallographic domains. Although those crystallographic defects are omnipresent in low-TT magnetite, the other defects may be additionally created by doping/nonstoichiometry. Our present results suggest that those kinds of defects pin trimerons in a more effective way than natural crystallographic domain walls do: BswB_{\mathrm{sw}} as well as UU, are higher for defected samples.

Axis switching is a relaxation process; i.e., it depends on the time the field is applied to the sample. At sufficiently low TT, the time of the axis change is long; in [13] the time dependence of magnetization was modeled and, using NMR, the authors showed that the AS process which at 57 K required even 24 h to complete. Because of this time dependence, in order to provide similar experimental conditions to draw BswB_{\mathrm{sw}} from mm vs BB, measuring time for each temperature should be adjusted accordingly. However, due to the time constraint this condition was not always fulfilled and the time of collecting the data was different for measurements at various temperatures. Nevertheless, the observation time does not challenge the fact that the trimeron system reacts to the external field much more readily in clean material than sluggishly as in doped samples. This fact justifies our estimation of all measured parameters in doped/nonstoichiometric samples; however the traces of this “time” problem are seen in our results. For example, this caused different mm vs BB slopes, visible, e.g., in Figure 4S(d) in SM [11]. It also affected BswB_{\mathrm{sw}} defined as the first BB value where m(B)m(B) was significantly off its value at T=4T = 4 K. All these contributed to the uncertainty of BswB_{\mathrm{sw}} (and, subsequently, Bi_swB_{\mathrm{i\_sw}}) estimation.

Checking AS dependence on dopant concentration mixes two effects: the defects’ impact on trimerons and the change of electronic structure these defects can cause. The effect of electronic structure on AS alone is probably better defined when hydrostatic pressure is exerted. This is seen in Figure 2-Figure 4, Figure 6, and Figure 7 and discussed below.

Pressure dependence of AS

The literature on magnetite properties consistently suggests that the system is highly sensitive to small differences in structural parameters, including those induced by pressure. For instance, studies have shown that applying pressure can lead to an increase in the Néel temperature [43], indicating a strengthening of the octahedral-tetrahedral exchange coupling, which is an important parameter in understanding the possible magnetic origin of the Verwey transition [14]. The temperature dependence of elastic constants has also been investigated under pressure, revealing a slight decrease in the coupling of the order parameter to strain [44,45]. Moreover, pressure has been found to have a significant impact on the local electron ordering in the ege_g and t2gt_{2g} orbitals, even at temperatures close to room temperature [46]. Many studies have focused on the influence of pressure on the Verwey transition, and it has been consistently observed that TVT_{\mathrm{V}} decreases gradually with increasing pressure for pressure values below 1.5 GPa in stoichiometric magnetite, nonstoichiometric magnetite, and Zn-doped ferrites2 [47,48,49,50] (see Fig. 13S(c) in SM [11] for some further results from the literature [51,52]).

Therefore, studying the influence of hydrostatic pressure on magnetite in the small range 0-1.2 GPa, could provide valuable insights into the peculiarities of AS and the subtle arrangement of orbital ordering.

It is important to note that applying pressure and subsequently releasing it does not leave the sample unchanged. The sample is different after a short stress which results, among other factors, in the increase of the TVT_{\mathrm{V}} under increasing impact strength, a still higher effect for more doped samples3 [54]. Application of pressure alters the electronic structure of the crystal by reduction of atom-atom distances and when pressure is released, this effect disappears. However, pressure may also affect the defect state which may be irreversible. Since TVT_{\mathrm{V}} lowering is universally observed when the sample is measured under hydrostatic pressure, we conclude that the change of electronic states and the ensuing effect on TVT_{\mathrm{V}} prevails over the effect of defects. This was also the reason we used rather small pressure, where the effects mentioned above are minute.

The main findings of our research are presented in Figure 2-Figure 4 (and in Fig. 12S in SM [11]). Additionally, pressure dependence of the switching field at representative temperatures (60 K for stoichiometric magnetite and 90 K for Zn-doped ferrite) is shown in Figure 6(a). BswB_{\mathrm{sw}} seems to decrease with increasing hydrostatic pressure both in stoichiometric and Zn-doped magnetite. In other words, when pressure is applied, BswB_{\mathrm{sw}} drops in a manner similar to the decrease in TVT_{\mathrm{V}}. A similar but less pronounced effect is observed in the AS energy EswE_{\mathrm{sw}} (Figure 3).

Taking a closer look to Figure 2, Figure 3 and Figure 6(a) (and 12S in SM [11]) it can however be noticed that after the initial drop of BswB_{\mathrm{sw}} and EswE_{\mathrm{sw}} from ambient pressure to p=0.37p = 0.37 GPa, both parameters stabilize with pp with a further decrease for p=1.2p = 1.2 GPa. Although it may be linked to some series of processes occurring under pressure, the uncertainty of data points collected under pressure p<0.8p < 0.8 GPa is rather high, and the unexpected phenomena take place at 1.2 GPa (see below). Therefore, the discussion of the subtleties in BswB_{\mathrm{sw}} and EswE_{\mathrm{sw}} vs pp is not justified and we only say that in general BswB_{\mathrm{sw}} seems to lower with pressure which is a general phenomenon in magnetite, independent of its doping character.

The factor that distinguishes stoichiometric and Zn-doped materials is the activation energy UU [Figs. 4 and 6(b)]. While pressure reduces UU in Zn-doped magnetite (resulting in a less temperature-dependent AS), the changes of UU for the stoichiometric sample are less evident, and there might even be a slight increase with pressure, although within a large range of error bars. Consequently, while UU shows a correlation with TVT_{\mathrm{V}} in Zn-doped magnetite (TVT_{\mathrm{V}} decreases with increasing xZnx_{\mathrm{Zn}}), some degree of anticorrelation is suggested for stoichiometric magnetite (including the region of very low pressure where TVT_{\mathrm{V}} appears to be at its maximum; see Fig. 13S(c) in SM [11]).

Hydrostatic pressure affects BswB_{\mathrm{sw}} and EswE_{\mathrm{sw}} in a similar manner to TVT_{\mathrm{V}}: all decrease with pressure. This stands in stark contrast to the impact of doping/nonstoichiometry, which leads to a considerable increase in BswB_{\mathrm{sw}} while causing TVT_{\mathrm{V}} to decrease. Therefore, the working hypothesis emerges that the mechanism responsible for TVT_{\mathrm{V}} lowering with dopants/nonstoichiometry is distinct from the mechanism behind TVT_{\mathrm{V}} lowering with pressure, as already formulated above.

As already outlined in Sec. 3, the process of defining an easy axis through field cooling is not entirely effective in stoichiometric magnetite under pressures of 1.2 GPa. In this case, the magnetic easy direction appears to be better defined after applying the magnetic field along the initially unspecified direction [10]. Since the results are much more controversial than for other pressure conditions, more is presented in Sec. 5(b) (Fig. 10S) of SM [11], while the main result is discussed here.

Figure 7 displays the magnetization curves at T=100T = 100 K along the “easy” direction [100] (after it was defined, as above, by field cooling with BB along [100]) and along the initially unspecified axis [10]. A comparison is made with m(B)m(B) curves along the easy axis [100] and unspecified [10] at T=10T = 10 K. It is evident that the two curves along [100] do not overlap, and the curve at T=100T = 100 K exhibits a hysteretic behavior, resembling the behavior observed after the AS process. However, the repeated m(B)m(B) scan along [100] is reproducible, indicating that no irreversible processes have occurred.

Interestingly, when the magnetization curve is measured along the initially unspecified direction [10], the AS process takes place, resulting in a final magnetization curve that resembles the "true" easy direction (depicted as the green curve in Figure 7). The phenomenon initiates at even lower temperatures (see Fig. 10S in SM [11] where the results at 100 and 70 K are compared) where the hysteretic behavior of m(B)m(B) along easy direction is less pronounced. A similar observation was made in a Zn-doped sample under pressure at 1.13 GPa and 105 K, as demonstrated in Fig. 11S(c) in SM [11], although this phenomenon was not extensively studied further.

In an attempt to comprehend the observed phenomena, several scenarios can be proposed. The prerequisite for the procedure used here to uniquely define the crystallographic cc and, simultaneously, magnetic easy axes was that electronic spins, manipulated by the external magnetic field, are so strictly confined to electronic states (i.e., also ionic arrangement) that the magnetic field uniquely defines the structure. This assumption, and the ensuing experimental procedure, were justified in ambient conditions but this may not be true at elevated pressure and high temperatures as our results show. A possible case is that either spins are less confined to the orbital moment (lower SOC), or orbital moment lowers with pressure, i.e., there is also magnetic field confinement to the ionic arrangement. Alternatively, magnetic axes no longer match crystallographic ones. In this last case, and assuming that the energy barrier between the “old” magnetic axes direction and “new” is not very high, the following explanation of the observed processes could be considered:

First, during the [100] field cooling, the structure still becomes uniquely defined, but magnetic anisotropy is smaller, resulting in a slightly different magnetic easy axis direction.

Second, magnetization vs BB along [100], although along the crystallographic cc axis, is along the axis that is not an easy magnetization axis and the magnetic domain structure is complicated and lacks saturation. However, for sufficient field (ca. 0.4-0.5 T) the saturation is achieved and the new energy minimum is realized. With field lowering, the magnetic system resides in this new energy minimum, even though the real one exists (but is separated by the energy barrier approximately proportional to the magnetic field) and is successively lowering: m(B)m(B) is different than on field rising.

Third, in zero field the magnetic system switches to the “old” minimum and the repeated m(B)m(B) is identical to the preceding one, as shown by the experiment (the red line in Figure 7).

Fourth, when mm vs BB is measured in the [10] direction, the m(B)m(B) curve is different than that along [100], eventually saturating in approximately the same field, but the saturation is realized by ionic changes, unlike along [100]. The argument for this is that the repetition of the same procedure gives different m(B)m(B) curve, much more similar to the “ideal” m(B)m(B) relation along the easy axis at ambient pressure. Note also that m(B)m(B) on lowering is more ideal than that along the [100] direction.

The proposed explanation: complicated and strongly magnetic field dependent magnetic structure should be further tested, as well as the possible structural changes under this pressure at TT close to TVT_{\mathrm{V}}.

The relation to magnetic anisotropy

The observed phenomena suggest that the magnetic anisotropy plays an important role in AS. In AS, electron orbitals in trimerons centers, which have more Fe2+^{2+} character are altered, likely due to the direct interaction of the magnetic field with orbital magnetic moment or the interaction of the magnetic field with spin, later transferred to the electronic orbital by SOC. All these seem to be closely linked to the magnetic anisotropy energy (EaE_{\mathrm{a}}). But magnetic anisotropy is only weakly temperature dependent [21, 19] [55] and marginally affected by small doping or nonstoichiometry (as seen in Fig. 15S in SM [11]), whereas AS exhibits significant changes under these conditions. Magnetic anisotropy involves placing the magnetic moments in a magnetic field which causes the reorganization of electronic states to lower their energy. This new energy under the magnetic field is higher anyway than without the field; therefore, finite energy is needed to rotate the magnetic moments. However, this process is reversible: once the magnetic field is removed, the electronic system returns to the initial state.

In the case of the processes studied here, if the energy rise of electronic states in the presence of magnetic field is higher than the barrier to an alternative electronic arrangement (in the form of trimerons), AS occurs. This AS process involves electron transfer leading to a new trimeron arrangement, accompanied by slight atomic displacements, ultimately resulting in a change in the cc-axis orientation. In the defected magnetite, whether through doping or nonstoichiometry, the electron transfer leading to a new trimeron arrangement becomes more challenging. In other words, defects increase the energy barrier preventing trimeron rearrangement, while the rigidity of the orbital/electronic order (linked to the anisotropy energy EaE_{\mathrm{a}}) remains largely constant. It is important to note that while magnetic anisotropy and axis switching are interconnected, they represent distinct phenomena.

The response to the external magnetic field was studied microscopically by observing individual Fe positions, including both the eight tetrahedral and 16 octahedral sites, using NMR [56], as well as groups of Fe positions using MS [12], all conducted under the influence of a magnetic field. The results demonstrated that the effective magnetic fields acting on Fe nuclei, both of isotropic and anisotropic character, change considerably with the direction of the magnetic field. Another aspect of these studies [56,57] highlights two groups of Fe BB positions (B1B1-B4B4 and B14B14 in one group and B7B7, B13B13, B16B16 in the other) that are highly sensitive to magnetic field compared to others. The calculated effective magnetic field in the first group [56] considerably decreases (by approximately 35%, compared to a maximum of 17% for other directions) when an external magnetic field is applied along <100><100>, different from the cc direction. Conversely, for the second group, the effective magnetic field considerably rises (again by 35%) under the same conditions. These two groups of atoms exhibit peculiar behaviors when observed by Mössbauer spectroscopy [34], all having relatively low valence (predominantly of Fe2+^{2+} character). Among them, five positions (C3) are trimeron centers, with one position, B14B14, also serving as a trimeron end point [1] [41]. In addition, all of these positions have a significant electric field gradient, much higher than other BB positions, the fact already mentioned in Secs. 4 a and 4 b above. These particular Fe positions are most sensitive to the effects of external field application along directions other than the cc-axis, indicating their involvement in the AS process. Once AS starts, electron charge transfer to other BB sites of Fe occurs, leading to trimeron reorganization. This charge transfer was observed in resistance vs magnetic field studies as spikes in resistance [58,59].

Conclusions

In summary, the mechanism of switching both the magnetic and cc monoclinic axes (abbreviated here as axis switching, AS), which essentially involves the reorganization of trimeron order, was studied by the observation of magnetic moment vs magnetic field behavior in stoichiometric, nonstoichiometric, and Zn-, Al-, and Ti-doped magnetite single crystals, in some cases also under hydrostatic pressure p<1.2p < 1.2 GPa. The level of doping and nonstoichiometry was kept below the highest values, xx and 3δ≤0.0123\delta\le0.012, which ensured that the discontinuous character of the Verwey transition remained unchanged, thus avoiding the introduction of additional phenomena. The results were quantified by phenomenological parameters: the switching field BswB_{\mathrm{sw}}, the activation energy UU, and the energy needed to switch the axis EswE_{\mathrm{sw}}.

Key findings from the studies include:

  1. BswB_{\mathrm{sw}} exhibits a significant increase when the defects, in the form of either nonstoichiometry or dopants, are introduced into the magnetite lattice. In stoichiometric and Zn-doped crystals, an increase in hydrostatic pressure (pp) leads to a decrease in BswB_{\mathrm{sw}}.

  1. A similar trend of increasing values with defects is observed for both the switching energy EswE_{\mathrm{sw}} and UU. However, UU shows an anticorrelation with TVT_{\mathrm{V}}, suggesting that AS and the decrease in TVT_{\mathrm{V}} vs. xx are not driven by the same microscopic mechanism. This is further supported by the fact that the work required to switch the axis is only on the order of 0.25 K per atom (and 0.05 K near TVT_{\mathrm{V}}), rather than around 50 K as reported in [2]. This indicates that some other trimeron excitations are observed here, and since the excitations in [2] are associated with the Verwey transition, the ones we observe are not.

  1. The application of pressure results in a lower value of UU for Zn-doped magnetite, whereas the effect of pressure on UU in stoichiometric magnetite is minor in comparison to the uncertainty of UU. Similarly, the uncertainty in EswE_{\mathrm{sw}} does not allow for a firm estimation of the Esw(p)E_{\mathrm{sw}}(p) trend, however slightly, suggesting that it decreases with pp.

  1. Both BswB_{\mathrm{sw}} and EswE_{\mathrm{sw}} decrease with increasing temperature across all the samples, but the application of pressure mitigates this effect. The response of specific iron BB sites to temperature and magnetic field direction, such as sites B1B1-B4B4 and B14B14, and B7B7, B13B13, B16B16, as observed by NMR [56], or group of sites (C3 group and C4 group, respectively) as seen by Mössbauer spectroscopy [34], are certainly connected with the processes observed in this study and strongly indicate that the electronic states in these sites are mainly responsible for the AS process.

  1. At pressures exceeding 0.8 GPa (particularly notable for x=0x = 0) there is an observable change of the electronic energy vs magnetic field landscape, which is reflected in the reversible hysteresis in mm vs BB relation, with BB oriented along the “easy axis” predefined by the field cooling. When mm is measured with BB increasing along a magnetically unspecified direction, the evident irreversible and hysteretic changes, similar to AS, occur. However, the resultant m(B)m(B) during decreasing BB is steeper than that for an easy axis. This suggests that the new direction becomes the ”better” easy axis compared to the one enforced by field cooling.

Acknowledgments

The work was supported by the National Science Centre, Poland, Grant No. OPUS: UMO-2021/41/B/ST3/03454, the Polish National Agency for Academic Exchange under “Polish Returns 2019” Programme: PPN/PP0/2019/1/00014, and the subsidy of the Ministry of Science and Higher Education of Poland. M.A.G., K.P., I.B., Z.K., and W.T. acknowledge the support from the “Excellence Initiative – Research University” program for AGH University of Krakow. I.B. acknowledges support from the Swiss Confederation through the Government Excellence Scholarship.

Supplemental Materials for:

Samples characterization and the effect of doping

Our aim was to see how a small disturbance of magnetite crystal alter the trimeron excitations. Therefore, we slightly doped magnetite with nonmagnetic dopants or introduced minute number of vacancies, as shown below [1, 20, 3, 4]:

Zn:≡Fe3−xZnxO4≡(Fe1−x3+Znx2+)[Fe1+x3+Fe1−x2+]O4\mathrm{Zn}: \equiv\mathrm{Fe}_{3-x}\mathrm{Zn}_{x}\mathrm{O}_{4} \equiv\left(\mathrm{Fe}_{1-x}^{3+}\mathrm{Zn}_{x}^{2+}\right)\left[\mathrm{Fe}_{1+x}^{3+}\mathrm{Fe}_{1-x}^{2+}\right]\mathrm{O}_{4}
Al:≡Fe3−xAlxO4≡(Fe1−0.15x3+Al0.15x3+)[Fe1−0.85x3+Fe2+Al0.85x3+]O4\mathrm{Al}: \equiv\mathrm{Fe}_{3-x}\mathrm{Al}_{x}\mathrm{O}_{4} \equiv\left(\mathrm{Fe}_{1-0.15x}^{3+}\mathrm{Al}_{0.15x}^{3+}\right)\left[\mathrm{Fe}_{1-0.85x}^{3+}\mathrm{Fe}^{2+}\mathrm{Al}_{0.85x}^{3+}\right]\mathrm{O}_{4}
Ti:≡Fe3−xTixO4≡(Fe3+)[Fe1−2x3+Fe1+x2+Tix4+]O4\mathrm{Ti}: \equiv\mathrm{Fe}_{3-x}\mathrm{Ti}_{x}\mathrm{O}_{4} \equiv\left(\mathrm{Fe}^{3+}\right)\left[\mathrm{Fe}_{1-2x}^{3+}\mathrm{Fe}_{1+x}^{2+}\mathrm{Ti}_{x}^{4+}\right]\mathrm{O}_{4}
Nonst.≡Fe3(1−δ)O4≡(Fe3+)[Fe1+6δ3+Fe1−9δ2+]O4\mathrm{Nonst.} \equiv\mathrm{Fe}_{3(1-\delta)}\mathrm{O}_{4} \equiv\left(\mathrm{Fe}^{3+}\right)\left[\mathrm{Fe}_{1+6\delta}^{3+}\mathrm{Fe}_{1-9\delta}^{2+}\right]\mathrm{O}_{4}

Here () denote tetrahedral (A) positions, while [] octahedral (B) ones. In the case of Al, this is the most probable alternative, although most probably Al3+^{3+} enters both octahedral and tetrahedral sites [4]. The influence of these disturbing species on the lattice is very small, yet different. For example, while Zn2+^{2+} (replacing Fe on A sites) and Ti4+^{4+} (on B sites) cations expand the lattice, Al3+^{3+} (entering both positions) shrinks it [5]. For lattice disturbance applied here this effect is, however, very small (ca. 0.01% for Zn and Al, possibly slightly larger for Ti), 10×\times lower than 1 GPa external pressure [22] used in case of our pressure studies. Contrary to this, the Verwey transition is a phenomenon vulnerable to even very small amount of spurious atoms, or nonstoichiometry as shown in Figure 1Sa and documented in vast literature, see e.g. [7, 8]. Already one third of a percent of Zn, Ti dopants or nonstoichiometry level changes the transition from discontinuous to continuous one and most studies claim that above 1% of doping the transition disappears completely. Note that this universal behavior is despite a fact that all those means to disturb the ideal structure enter this structure in a different way and with the different valence. The problem why a small amount of dopands/nonstoichiometry universally affect the transition is still not resolved although we have shown [9, 10] that the excitation spectrum, observed with specific heat, is drastically different for two regimes of the Verwey transition. Note, finally, that in case of other dopants, e.g. Al used in this work, the effect of doping on VT is less acute (Figure 1Sa) and does not obey the universal TVT_{\mathrm{V}} vs. x=3δx=3\delta relation.

Image not extracted

Figure 1S. (a) Universal TVT_V vs. xx, 3δ3\delta relation (for nonstoichiometric as well as Zn, Al, and Ti doped magnetite [1, 20, 3, 4]). The data for Ga, Ni, Co, Mg doping are cited after [23]. Samples measured here are shown with large symbols (full in case measured under pressure). (b) Magnetic AC susceptibility vs. temperature for all measured samples.

The majority of the samples used in this study were cylindrical in shape, with a typical diameter of 2-3 mm and similar length, except for the measurements conducted under pressure, where the diameter was approximately 1 mm. The crystals were first oriented using Laue diffraction and subsequently polished with the long cylinder axis oriented along [1] cubic direction with the accuracy higher than 2 degrees. Since no further Laue check was performed after polishing the samples into cylinder, the direction mismatch of up to 3 degrees can be expected. Additionally, a spherical-shaped sample with diameter of 2.5 mm was oriented after its preparation.

The Verwey transition temperature of the samples was estimated from magnetic susceptibility χAC\chi_{\mathrm{AC}} vs. TT relation, shown in Figure 1Sb. Zn, Ti, and Al content was estimated from the universal TVT_V vs. xx dependence presented in Figure 1Sa, while the nonstoichiometry parameter δ\delta in Fe3(1−δ)O4\mathrm{Fe}_{3(1-\delta)}\mathrm{O}_4 was set upon annealing.

Efficacy of field cooling in easy axis determination

The prerequisite in all experiments presented in the main text and SI is that cc crystallographic and, simultaneously, magnetic easy axes are uniquely defined by field cooling with BB along one of cubic ⟨100⟩\langle100\rangle directions. Therefore, the check how large the cooling field should be was a first part of our studies. In case the axes are not uniquely defined magnetic moment vs. BB, m(B)m(B), along this axis is not typical for an easy axis direction and should show irreversible changes. In Figure 2Sa, m(B)m(B) are presented after field cooling in several fields showing that the sample should be cooled in at least 0.25 T field to set the easy axis.

However, field application (0.9 T) along one of ⟨100⟩\langle100\rangle axes below TVT_V, e.g. at 80 K, also sets an easy axis in this direction (this is AS studied here), even though both processes (field cooling and forcing an easy axis at T<TVT < T_V) are different. In Figure 2Sb, the comparison of the results (FC and 0.9 T field application after ZFC to 80 K) are presented. This shows that second process (bulk squares; it is supposed to define an easy axis along [100]) is almost as effective in easy axis determination as the field cooling in 0.25 T (triangles), or 0.25 T field cooling followed by field application along the same axis (open squares). Note, however, that slightly larger field is needed to complete AS in the first case (after ZFC and subsequent 0.9 T field application at T<TVT < T_{\mathrm{V}}); this is presented in Figure 2Sb. To assure that both ways to define easy (and cc) axis lead to the same result, in all the studies presented in this paper, 0.9 T cooling field was used.

Image not extracted

Figure 2S. Efficacy of field cooling and field application below TVT_{\mathrm{V}} in establishing the cc and, simultaneously, easy magnetic axes. Field cooling in different fields along [100] defines, Fig. 2Sa, the easy axis (and cc crystallographic axis) above FC 0.25 T (starting from FC 0.2 T, mm vs. BB curves start to be identical to an easy direction case). Field cooling along [100] and 0.9 T field application along [100] at 80 K after ZFC have almost equal effect although slightly larger field is needed to complete AS in the first case (Figure 2Sb).

Pressure experiments

The samples for pressure experiments (stoichiometric Fe3_3O4_4 #3 and Zn doped, xZn=0.0066x_{\mathrm{Zn}} = 0.0066) were the long rods, (ca. 5 mm length, 0.8 mm diameter) cut with long rod axis along [100] direction. The samples were first loaded to the nonmagnetic (CuBe) cell filled with silicon oil (pressure transmitting medium) with a tiny piece of tin separated from the sample with nonmagnetic separating rod (Figure 3S). Then, the cell was pressed to appropriate pressure (shown by the gauge), secured with the nut and attached to the measuring rod of VSM. The exact pressure was read from the superconducting tin transition (TC<4T_{\mathrm{C}} < 4 K, i.e. below the typical temperatures the samples were measured). The details of the pressure cell are described elsewhere [12].

Image not extracted

Figure 3S. Pressure cell used in magnetization vs. pressure measurements. The pressure value was checked against pressure dependent superconducting transition in tin.

Results of mm vs. BB experiments under ambient pressure

Stoichiometric and nonstoichiometric magnetite

Nine-panel plot of $m(B)$ and related quantities for stoichiometric and nonstoichiometric magnetite

Figure 4S. m(B)m(B) for stoichiometric magnetite below TVT_{\mathrm{V}} along unspecified direction showing AS (a, c, d), and ensuing fit to Calhoun’s relation (e, g, h). In panels b and f m(B)m(B) for Fe3_3O4_4 #2 at 290 K, along ⟨100⟩\langle100\rangle, hard above TVT_{\mathrm{V}}, and ⟨011⟩\langle011\rangle, intermediate above TVT_{\mathrm{V}} are presented. The difference between ⟨100⟩\langle100\rangle and ⟨011⟩\langle011\rangle are best seen in field of ca. 0.15-0.2 T. The minimum in mm vs. vector BB direction is along [100]. In case of Fe3_3O4_4 #3, also

temperature dependence of the energy needed to switch the cc axis, EswE_{\mathrm{sw}}, as well as the temperature dependence of Bi,swB_{i,\mathrm{sw}} are shown (panel i).

Nonstoichiometric Fe3(1−δ)O4\mathrm{Fe}_{3(1-\delta)}\mathrm{O}_{4} magnetite

Magnetization curves and switching-energy temperature dependence for nonstoichiometric magnetite

Figure 5S. Same as in Fig. 4S but for nonstoichiometric samples. All the curves, except the indicated one, are along unspecified axis and show AS.

Zn, Al, and Ti doped magnetite

m(B) curves and fits for Zn-, Al-, and Ti-doped magnetite samples

Figure 6S. m(B)m(B) (panels a-e) and fits to Calhoun’s relation (f-j) for doped samples in ambient pressure. Since the data for Ti doped sample are of lower quality, in this case also those m(B)m(B) curves where BswB_{\mathrm{sw}} estimation was not possible are presented. Note also that the uncertainty of UU is, in this case, large, unlike in other samples.

In Figure 7S the TT dependence of switching field and energy needed to switch the axis for all measured samples under ambient pressure are shown.

Figure 7S. TT dependence of switching field (a) and energy needed to switch the axis (b) of all measured samples under ambient pressure.

Sample training experiment

Axis switching is an activation-type phenomenon, as is clear both from old [13] and our [14, 15] studies. It is thus important to check how repeatable this process is and how it depends on the measurement procedure. We have performed AS five times, after the single field cooling along [100] direction, with the field first directed along [10], then [100], etc. Each time AS occurred, magnetic field direction became a new the cc axis that could be again switched by repeated field application. The results of this sample training, for a representative temperature (80 K and 100 K), fitting to the Calhoun’s formula and Bi,swB_{\mathrm{i,sw}} vs. TT for three successive runs are shown in Fig. 8S. This is clear that switching fields are highest for the first switching event and are lower, and almost constant, in subsequent switching, while temperature dependence of it (expressed by the activation energy UU) stays constant (U/kBU/k_B = 364 K, 357 K, 329 K, all within the error bar of ca 50 K; this is presented in Fig. 8Sc).

The results from these experiments, i.e. the decrease of switching field with no considerable changes of UU, show that these two parameters are not straightforwardly coupled as Calhoun’s formula suggests. In other words, defects caused by AS decrease BswB_{\mathrm{sw}} without affecting the barrier the charges (and ions in a slight ionic rearrangement) must cross. UU also measures how the process reacts to the changes of temperature; the result suggests that smaller field is needed to trigger AS, but the pace it changes with TT and the barrier are the same. The most important outcome of this experiment is that AS introduces some changes to the system (“AS defects”) that act unlike dopants/nonstoichiometry do.

Figure 8S. Sample training. Panels a and b: selected data of mm vs. BB from which Bi,swB_{\mathrm{i,sw}} vs. TT and UU were calculated. In each case, the sample was first FC in 0.5 T along [100] and then m(B)m(B) was measured along [10] setting this as an easy axis. The sample was then rotated 90° (to an unspecified axis) and the procedure m(B)m(B) was repeated (“2 run”). The procedure was repeated 4 (panel a) or 5 times (panel b). Fitting to Calhoun’s formula is presented in panel c, while switching field vs. temperature during the sample training is in panel d.

Results of pressure experiments

m(B)m(B) experiments for stoichiometric Fe3O4\mathrm{Fe}_{3}\mathrm{O}_{4} #3

Since samples had slightly lower diameters than the sample chamber (this is shown in the scheme of the pressure cell in Figure 3S) some movement in silicon oil was possible and was observed. Therefore, as already remarked in the main text, the procedure to find cubic hard (easy below TVT_{\mathrm{V}}) and intermediate directions was done at 160 K to allow pressure transmitting medium to freeze. Also, the size incompatibility could result in some skew of the sample axis and, consequently, in some difference between magnetic moment in two perpendicular directions. This problem, although noticed in some cases, is not further discussed.

Pressure measurements of stoichiometric Fe3O4 #3

Figure 9S. The results of pressure (a, b, c) measurements of the stoichiometric sample Fe3O4\mathrm{Fe}_{3}\mathrm{O}_{4} #3 (the data under ambient pressure are presented in Figure 4Sd and Figure 4Sh). In panels d, e, f ln⁡(Bi_sw/T)\ln(B_{i\_sw}/T) vs. 1000/TT and ensuing UU values are shown. Since for p=1.2p = 1.2 GPa the clear scheme of [100] as an easy axis and [10] as an unspecified one starts to be uncertain, mm vs. BB for both directions are presented.

Monoclinic cc and magnetic easy axes cannot be simultaneously set for Fe3_3O4_4 #3

As mentioned in the main part, the procedure to set an easy direction along cooling field was effective in case p=1.2p = 1.2 GPa and for x=0x = 0 at lower TT below 65 K. However, at higher temperatures, above 70 K, magnetic moment m(B)m(B) along [100] (supposed to become an easy axis after FC) did not show typical results as for an easy axis.

This is presented in Fig. 10Sa at 70 K and compared to the usual behavior (an unspecified [10] at 10 K and an easy direction [100] at 30 K under ambient pressure). There is a hysteresis at 70 K in m(B)m(B) along “easy” [100] (but reversible, as discussed in the main text), but m(B)m(B) along [10] shows the process similar to AS with m(B)m(B) under lowering BB steeper than an “easy” axis. The repeated m(B)m(B) along the same direction (it should be on the same line if AS were completed) is slightly different as if the easy axis was “strengthened”.

The effect is more visible at higher temperatures what Fig. 10Sb shows. In particular m(B)m(B) at 100 K on field rising for an unspecified [10] is steeper than for “easy” [100] direction.

Magnetization process of stoichiometric sample Fe$_3$O$_4$ #3 under pressure of 1.2 GPa at temperatures above 65 K, shown in panels (a) and (b)

Figure 10S. Magnetization process of stoichiometric sample Fe3_3O4_4 #3 under pressure of 1.2 GPa and at T>65T > 65 K showing different than in other cases behavior. First, panel a, m(B)m(B), along the “easy” [100] shows hysteresis, increasing at higher temperatures (panel b) and reversible (Figure 7 in the main text) when repeated. Second, m(B)m(B) along “unspecified” [10] also shows hysteresis that is non reversible (panel a: red and blue symbols). Note that m(B)m(B) on BB lowering is steeper along [10] (i.e. after “axis switching”) than along the “easy axis” [100]. The process increases at higher temperatures as panel b and Figure 7 in the main text show.

m(B)m(B) experiments for Fe3−xZnxO4\mathrm{Fe}_{3-x}\mathrm{Zn}_{x}\mathrm{O}_{4} Zn#3

Results of ambient and pressure measurements of the Zn doped sample

Figure 11S. The results of ambient (a, d) and pressure (b, c, e, f) measurements of the Zn doped sample and fittings to Calhoun’s relation. Note, panel c, that ill-defined easy axis starts to be visible also in Zn doped sample under pressure 1.13 GPa at 105 K.

Pressure impact on energies and BswB_{\mathrm{sw}}

In Figs. 12Sa, b the same parameters as in the main text are presented but focused only on dependence on pressure.

Temperature dependence of the switching field, energy needed to switch the axis, and correlation of activation energy with the Verwey temperature

Figure 12S. Temperature dependence of the switching field (a), energy needed to switch the axis (b) and the correlation of activation energy with the Verwey temperature (c) for both samples measured under elevated pressure.

TVT_{\mathrm{V}} dependence on pressure

The measurements were performed in non-saturation field and were solely aimed on TVT_{\mathrm{V}} vs. pp check. Note that the TVT_{\mathrm{V}} for p=0p = 0 was not recorded but was drawn from susceptibility measurements. In any case, our result confirms the result from [52] of a possible initial rise in TVT_{\mathrm{V}} vs. pp.

Figure 13S. TVT_{\mathrm{V}} vs. pressure for measured samples and the literature data. In present studies TVT_{\mathrm{V}} was drawn from magnetic moment vs. TT dependence on heating (panels a and b). In panel c those TVT_{\mathrm{V}} values (stars) are superimposed on the literature data of low pressure impact on Verwey transition temperature (1: [16] 2: [51], 3: [18], 4: [52]).

Pressure dependence of magnetic moment

The important information presented in the literature few years ago concerned the change of spinel structure under pressure: it was suggested in [25, 26, 27, 28] that apart from the Verwey transition there is also a transition from high TT inverse spinel to the low TT normal spinel lattice [Fe2+]TET[Fe3+Fe3+]OCT\left[\mathrm{Fe}^{2+}\right]_{\mathrm{TET}}\left[\mathrm{Fe}^{3+}\mathrm{Fe}^{3+}\right]_{\mathrm{OCT}} that proceeds at the same temperature TCC=TVT_{\mathrm{CC}} = T_{\mathrm{V}} as the Verwey transition under ambient pressure, but with TCCT_{\mathrm{CC}} growing when pressure is increased. Such coordination crossover should result in a drastic (20%) change of saturation magnetic moment vs. TT relation. Although some contortions in MsM_{\mathrm{s}} vs. TT are present, 5%, at most, (Fig. 14S) the pronounced changes were not found in our results. Thus, in agreement with other literature [29, 30], our data question the exact character of inverse to normal spinel transition. However, since we see an unexpected behavior of the magnetic easy axis, as commented in the main text, some processes under pressure certainly take place possibly related to the recently mentioned changeover in cation presence in A and B positions [31].

Saturation moment versus temperature for studied samples

Figure 14S. Saturation moment mSm_{\mathrm{S}} vs. TT for studied samples. No major change of mSm_{\mathrm{S}} was found that refutes claims of the pressure-induced change from low-TT normal to high-TT inverse spinel at TCCT_{\mathrm{CC}} (shown in the inset; here red line limits the pp range covered here).

Magnetic anisotropy energy

Figure 15S. Magnetic anisotropy energy for stoichiometric, nonstoichiometric, Ti doped and Zn doped magnetite (based on [1, 3, 27]).

Relation to magnetic anisotropy

Axis switching is linked with magnetic anisotropy. Therefore, the temperature dependence of magnetic anisotropy drawn from published literature data is presented in Fig. 15S.

Additional information on the temperature dependence of AS

Several phenomena can be considered that trigger temperature dependence of AS.

First, it was suggested that spin-orbit coupling may depend on TT [33]. In the case of such situation, the spins in octahedral positions might gradually increase their coupling to electronic orbitals. This coupling may culminate in some magnetic field and at some temperature in a coupled spins and orbitals reconfiguration, i.e. AS. However, this should presumably be linked to some increase of saturation magnetic moment in magnetite below TVT_{\mathrm{V}} (that would result from orbital moment alignment along magnetic field), the phenomenon never observed. We therefore consider this mechanism of AS temperature dependence as rather improbable.

The next species that certainly change with temperature are lattice vibrations. Although phonon DOS does not seem to be TT-dependent and even the change of it at TVT_{\mathrm{V}} is not very pronounced [10] [35], it is natural to suspect that increasing the amplitude of atomic vibrations should increase the probability of AS and also lower BswB_{\mathrm{sw}}. Since vibration amplitude has roughly square root dependence in TT, the same dependence should characterize BswB_{\mathrm{sw}} vs. TT. However, BswB_{\mathrm{sw}} vs. TT has an activation, exponential, character already used by us for activation energy UU estimation. Thus, phonons alone cannot be mainly responsible for the phenomenon we observe.

Finally, AS and its change with temperature can be related to 8 octahedral Fe positions, B4, B14, B3, B2 and B1, and B7, B13 and B16 (see [34] for the reference to Fe sites labeling), which are grouped into components C3 and C4, respectively, in the Mössbauer spectrum of stoichiometric and Zn-doped magnetite [34]. Atoms in these two groups experience a particularly large decrease in the electric field gradient VzzV_{zz} with TT below TVT_{\mathrm{V}}. There is also a large change in VzzV_{zz} for these sites when Zn doping exceeds the first order transition limit, with the sign of VzzV_{zz} even reversed for the C3 group and a simultaneous increase in temperature dependence. Of these positions, one group, C4, has lower BeffB_{\mathrm{eff}} (36 T compared to about 50 T for other groups) and both groups have the lowest valence, close to 2+ (the highest isomer shift parameter). Also, both groups are peculiar in the sense that their anisotropic component of BeffB_{\mathrm{eff}} is relatively high and the isotropic component low, in contrast to other positions, and that a sharp decrease of BeffB_{\mathrm{eff}} with TT is seen for C4 at higher Zn contents. All this suggests that a strong T dependence of AS may be somehow related to these B positions.

References

  1. [1]J. W. Koenitzer, Magnetization studies of zinc-substituted magnetite, PhD Thesis, Purdue University, 1992.
  2. [2]Z. Kąkol, J. Sabol, and J. M. Honig, Cation distribution and magnetic properties of titanomagnetites, Phys. Rev. B 43, 649 (1991).
  3. [3]Z. Kąkol, and J. M. Honig, Influence of deviations from ideal stoichiometry on the anisotropy parameters of magnetite Fe₃₍₁₋δ₎O₄, Phys. Rev. B 40, 9090 (1989).pubmed.ncbi.nlm.nih.gov/9991395
  4. [4]A. Kozłowski, P. Metcalf, Z. Kąkol, and J. M. Honig, Electrical and magnetic properties of Fe₃₋ₓAlₓO₄, x < 0.06, Phys. Rev. B 53, 15113 (1996).
  5. [5]Z. Kąkol, D. Owoc, J. Przewoźnik, M. Sikora, C. Kapusta, D. Zając, A. Kozłowski, J. E. Sabol, and J. M. Honig, The effect of doping on global lattice properties of magnetite Fe₃₋ₓMeₓO₄ (Me=Zn, Ti, and Al), J Solid State Chem. 192, 120 (2012).DOI
  6. [6]A. Kuriki, Y. Moritomo, Y. Ohishi, K. Kato, E. Nishibori, M. Takata, M. Sakata, N. Hamada, S. Todo, N. Mori, O. Shimomura, and A. Nakamura, High-Pressure Structural Analysis of Fe₃O₄, J. Phys. Soc Jpn, 71, 3092 (2002).DOI
  7. [7]Z. Kąkol, A. Kozłowski, T. Kołodziej, and J. Przewoźnik, Charge rearrangement in magnetite: from magnetic field induced easy axis switching to femtoseconds electronic processes, Phil. Mag. 95, 633 (2015).DOI
  8. [8]J. M. Honig, Analysis of the Verwey transition in magnetite, J. All. Compd. 229, 24 (1995).DOI
  9. [9]A. Kozłowski, Z. Kąkol, D. Kim, R. Zalecki, and J. M. Honig, Heat Capacity of Fe₃₋ₓMₓO₄, M=Zn, Ti, 0 ≤ x ≤ 0.04, Phys. Rev. B 54, 12093 (1996).
  10. [10]T. Kołodziej, A. Kozłowski, P. Piekarz, W. Tabiś, Z. Kąkol, M. Zając, Z. Tarnawski, J. M. Honig, A. M. Oleś, and K. Parliński, Nuclear inelastic scattering studies of lattice dynamics in magnetite with a first- and second-order Verwey transition, Phys. Rev. B 85, 104301 (2012).DOI
  11. [11]V. A. M. Brabers, F. Walz, and H. Kronmüller, Impurity effects upon the Verwey transition in magnetite, Phys. Rev. B 58 14163 (1998).DOI
  12. [12]M. Baran, V. Dyakonov, L. Gladczuk, G. Levchenko, S. Piechota, and H. Szymczak, Comparative study of the pressure effect on critical parameters of GdBa₂Cu₄O₈ and YBa₂Cu₄O₈, Physica C 241, 383 (1995).
  13. [13]B. A. Calhoun, Magnetic and Electric Properties of Magnetite at Low Temperatures, Phys. Rev. 94, 1577 (1954).DOI
  14. [14]G. Król, J. Kusz, Z. Tarnawski, Z. Kąkol, W. Tabiś, and A. Kozłowski, Studies of the magnetic axis switching in magnetite, Acta Phys. Pol. A 109, 601 (2006).DOI
  15. [15]V. Chlan, K. Kouřil, H. Štěpánková, R. Řezníček, J. Štěpánek, W. Tabiś, G. Król, Z. Tarnawski, Z. Kąkol, and A. Kozłowski, Magnetically induced structural reorientation in magnetite studied by nuclear magnetic resonance, J. Appl. Phys. 108, 083914 (2010).DOI
  16. [16]Y. Kakudate, N. Mori, and Y. Kino, Pressure effect on the anomalous electrical conductivity of magnetite, J. Magn. Magn. Mater. 12, 22 (1979).DOI
  17. [17]S. Tamura, Pressure Dependence of the Verwey Temperature of Fe₃₋ᵧO₄ Obtained by Magnetic Permeability Measurements, J. Phys. Soc. Jap. 59, 4462 (1990).DOI
  18. [18]G. K. Rozenberg, G. R. Hearne, and M. P. Pasternak, Nature of the Verwey transition in magnetite (Fe₃O₄) to pressures of 16 GPa, Phys. Rev. B 53, 6482 (1996).pubmed.ncbi.nlm.nih.gov/9982047
  19. [19]A. Wiecheć, R. Zach, Z. Kąkol, Z. Tarnawski, A. Kozłowski, and J. M. Honig, Magnetic Susceptibility Studies of Single Crystalline Zinc Ferrites Under Pressure, Physica B 359-361, 1342 (2005).DOI
  20. [20]G. Kh. Rozenberg, Y. Amiel, W. M. Xu, M. P. Pasternak, R. Jeanloz, M. Hanfland, and R. D. Taylor, Structural characterization of temperature- and pressure-induced inverse↔normal spinel transformation in magnetite, Phys. Rev. B 75, 020102(R) (2007).DOI
  21. [21]M. P. Pasternak, W. M. Xua, G. Kh. Rozenberg, R. D. Taylor, and R. Jeanloz, Pressure-induced coordination crossover in magnetite, a high pressure Mössbauer study, J. Phys. Chem. Solids 65, 1531 (2004).DOI
  22. [22]M. P. Pasternak, W. M. Xua, G. Kh. Rozenberg, R. D. Taylor, and R. Jeanloz, Pressure-induced coordination crossover in magnetite; the breakdown of the Verwey–Mott localization hypothesis, J. Magn. Magn. Mater. 265, L107 (2003).DOI
  23. [23]G. Kh. Rozenberg, M. P. Pasternak, W. M. Xu, Y. Amiel, M. Hanfland, M. Amboage, R. D. Taylor, and R. Jeanloz, Origin of the Verwey transition in magnetite, Phys. Rev. Lett. 96, 045705 (2006).pubmed.ncbi.nlm.nih.gov/16486848
  24. [24]H. Kobayashi, I. Isogai, T. Kamimura, N. Hamada, H. Onodera, S. Todo, and N. Môri, Structural properties of magnetite under high pressure studied by Mössbauer spectroscopy, Phys. Rev. B 73, 104110 (2006).DOI
  25. [25]S. Klotz, G. Rousse, Th. Strässle, C. L. Bull, and M. Guthrie, Nuclear and magnetic structure of magnetite under pressure to 5.3 GPa and at low temperatures to 130 K by neutron scattering, Phys. Rev. B 74, 012410 (2006).DOI
  26. [26]H. Elnaggar, S. Graas, S. Lafuerza, B. Detlefs, W. Tabiś, M. A. Gala, A. Ismail, A. van der Eerden, M. Sikora, J. M. Honig et al., Temperature-Driven Self-Doping in Magnetite, Phys. Rev. Lett. 127, 186402 (2021).DOI
  27. [27]Z. Kąkol, J. Sabol, J. Stickler, A. Kozłowski, and J. M. Honig, Influence of Titanium Doping on the Magnetocrystalline Anisotropy of Magnetite, Phys. Rev. B 49, 12767 (1994).pubmed.ncbi.nlm.nih.gov/10010181
  28. [28]L. Zhang, Y. B. Chen, B. Zhang, J. Zhou, S. Zhang, Z. Gu, S. Yao, and Y. Chen, Sensitively Temperature-Dependent Spin–Orbit Coupling in SrIrO₃ Thin Films, J. Phys. Soc. Jpn. 83, 054707 (2014).DOI
  29. [29]P. Piękarz, D. Legut, E. Baldini, C. A. Belvin, T. Kołodziej, W. Tabiś, A. Kozłowski, Z. Kakoł, Z. Tarnawski, J. Lorenzana, N. Gedik, A. M. Oleś, J. M. Honig, and K. Parliński, Trimeron-phonon coupling in magnetite, Phys. Rev. B 103, 104303 (2021).DOI
  30. [30]V. Chlan, J. Žukrowski, A. Bosak, Z. Kakoł, A. Kozłowski, Z. Tarnawski, R. Řezníček, H. Štěpánková, P. Novák, I. Biało, and J. M. Honig, Effect of low Zn doping on the Verwey transition in magnetite single crystals: Mössbauer spectroscopy and x-ray diffraction, Phys. Rev. B 98, 125138 (2018).DOI

Paper details

vlnc:W_2r9khk2x
Version
v1 · latest
Published
Fresh — added to the Hub within the last 30 days
Added
License
CC BY 4.0
Usage

views · 0

downloads · 0

A view counts once per browser per day, a download each time the PDF is requested.

  • Physics and Astronomy

Not recorded for this paper

View statement
Looking for related papers…
Contents