Epitaxial growth of WO3 on r-plane sapphire by hot-filament metal-oxide deposition using CO2 as a precursor

Abstract

The deposition of epitaxial films of WO3 by hot-filament metal-oxide deposition using CO2 as a precursor was demonstrated. The films were obtained at a low growth rate of 0.25 nm/min. The optical properties of the film were assessed by variable-angle spectroscopic ellipsometry, indicating transparency across the visible spectrum and high absorption above 3 eV.

Introduction

Tungsten trioxide, denoted WOx\mathrm{WO}_x with 2<x≤32 < x \le3 is a versatile multifunctional material with a large compositional homogeneity ranges, and a variety of crystal structures.[1, 2] The properties of interest range from semiconducting behavior with tunable bandgap, thermochromicity[3], electrochromicity[3, 4], photochromicity[5], ferroelectricity[6], superconductivity, gas detection[7, 8, 9] and template for transition metal dichalcogenide growth[10]. Synthesis of WOx\mathrm{WO}_x has been achieved by a range of physical[7, 8, 11, 12, 13, 14, 15, 16, 17, 18, 19, 20] and chemical[6, 9, 10, 21, 22, 23, 24, 25, 26] vapor deposition techniques. One common approach to the synthesis of WOx\mathrm{WO}_x is the hot-filament metal oxide deposition (HFMOD) method.[11, 12, 17, 18, 19, 20] The method relies on the oxidation[27, 28, 29, 30] of a hot tungsten wire by flowing O2\mathrm{O}_2[17, 18], H2O\mathrm{H}_2\mathrm{O}[19] or air[11, 12, 17, 20], and on the volatility of the oxides formed.[31]

Here, we instead use CO2\mathrm{CO}_2 as oxidizing species. CO2\mathrm{CO}_2 has long been known as an oxidizing agent of W, for example in reducing the lifetime of tungsten filaments in incandescent lamps[32, 33] and in gas sensing[28]. Besides the advantage of upcycling a major greenhouse gas into valuable materials, CO2\mathrm{CO}_2 is a much milder oxidizer[28] than O2\mathrm{O}_2 or H2O\mathrm{H}_2\mathrm{O}. Furthermore, the formation of carbon monoxide (CO) as a byproduct of oxidation of the wires is expected to provide an additional means to tune the composition as it can act as a reducing agent for WOx\mathrm{WO}_x. This role of CO has been demonstrated in the case of the molybdenum oxides[34], and offers a means of engineering the composition and ultimately the properties of the deposited tungsten oxides. Thus, we here demonstrate epitaxial growth of orthorhombic (oo-) or monoclinic (mm-) WO3\mathrm{WO}_3 on r-plane sapphire by HFMOD using CO2\mathrm{CO}_2 as oxidizing gas.

Experimental details

Tungsten oxide thin films were deposited onto r-plane sapphire substrates (α\alpha-Al2O3\mathrm{Al}_2\mathrm{O}_3(012), Alineason) in a hot-filament CVD (HFCVD) reactor (Blue Wave Semiconductors BWI 1000 HFCVD) by the reaction of tungsten (2 wires, 0.5-mm diameter, 8-cm long, 99.95% purity) with CO2\mathrm{CO}_2 (99.998% purity). The wires were placed at an average distance of 25 mm from the substrates.

The substrates were sonicated in acetone, isopropanol, and deionized water for 5 min each, then blow-dried using N2\mathrm{N}_2 and loaded in an alumina crucible into a crucible furnace. The substrates were annealed in ambient air at 1000 °C for 60 min, with a temperature ramp-up of 5.4 °C/min and a passive cooldown. The substrates were stored in air no longer than three days.

Prior to loading into the HFCVD chamber, the substrates were sonicated once more in acetone and isopropanol for 5 min each, blow-dried using N2\mathrm{N}_2. The base pressure of the system before deposition was <4.0×10−5< 4.0 \times10^{-5} Pa (3.0 ×10−7\times10^{-7} Torr). The depositions were run using 10 SCCM CO2\mathrm{CO}_2, resulting in a pressure of 7.2×10−27.2 \times10^{-2} Pa (5.4 ×10−4\times10^{-4} Torr), at a substrate temperature of 450 °C, for 30-120 min, and with the substrate rotating at a speed of 12.5 rpm. Argon (Ar, 99.999%) was used at the same partial pressure of 7.2×10−27.2 \times10^{-2} Pa as a substitute to CO2\mathrm{CO}_2 to dismiss the role of impurities (O2\mathrm{O}_2, residual H2O\mathrm{H}_2\mathrm{O}) as potential oxidizers. The total current through the filaments was 35 A (17.5 A per filament). The corresponding filament temperature was estimated using the following equation:

T=(PJouleϵWσA+T04)14=(ρ(T)I22π2r3ϵWσN+T04)14,(1)T = \left(\frac{P_{\mathrm{Joule}}}{\epsilon_{\mathrm{W}}\sigma A} + T_0^4\right)^{\frac{1}{4}} = \left(\frac{\rho(T)I^2}{2\pi^2r^3\epsilon_{\mathrm{W}}\sigma N} + T_0^4\right)^{\frac{1}{4}}, \tag*{(1)}

where TT is the temperature of the wire, T0T_0 is the room temperature, PJouleP_{\mathrm{Joule}} is the power dissipated as heat by a resistor, εW\varepsilon_W is the emissivity of tungsten which we assumed constant and equal to 0.46 [35], σ\sigma is the Stefan-Boltzmann constant, AA is the total emitting area, II is the total current running through the filaments, rr is the radius of a filament and NN the number of identical filaments. The dependence of the resistivity of tungsten in the range 2000 to 3600 K is given by[36]:

ρ(T)=(−14.08+0.03515T)×10−8 [Ω.m](2)\rho(T) = (-14.08 + 0.03515T) \times10^{-8}\,[\Omega.\mathrm{m}] \tag*{(2)}

which after 6 iterations of equations (1) and (2) converges to T=2220T = 2220 K (1947 °C).

X-ray diffraction (XRD) was measured using Cu Kα\alpha radiation. XRD 2θ/ω2\theta/\omega scans were recorded on a PANalytical Empyrean diffractometer with the integrated module iCore (Bragg-Brentano HD graded mirror with 0.8° acceptance angle, 0.03 rad Soller slits, 0.5° divergence slit at a sample distance of 96 mm) on the primary side and the integrated module dCore (17 mm anti-scatter slit, 0.02 rad Soller slits, 0.28° Parallel plate collimator) and PICel3D-Medipix3 detector on the secondary side. GID (Glancing incidence glancing exit diffraction) scans and X-ray pole figure were recorded on a X’Pert MRD diffractometer. A capillary lens with cross-slits was used on the primary side and a 0.18° parallel plate collimator and proportional detector were used on the secondary side, the cross-slits were set to 2×22 \times2 mm2^2 for pole figure measurement and 8×28 \times2 mm2^2 for GID measurements.

Variable-angle spectroscopic ellipsometry (VASE, RC2-XI Woollam) was used to evaluate the thickness and optical properties of the deposited films. The measurements were performed at incident angles of 50°, 55° and 60° of the range 0.73-5.9 eV. The data was modelled and fit using the CompleteEASE software (6.51).

Results and discussion

Figure 1(a) shows 2θ/ω2\theta/\omega scans from films deposited with CO2\mathrm{CO}_2 for 30 min and 120 min, and for comparison films deposited with pure Ar. The XRD scan from the film deposited with CO2\mathrm{CO}_2 for 30 min exhibits distinct Laue fringes (Figure 1(b)), meaning that films of high crystalline quality are obtained. The fringes for the films deposited for 120 min are difficult to resolve because of their higher thickness of 30 nm, as measured by ellipsometry, corresponding to an average growth rate of 0.25 nm/min.

Extended 2θ/ω scans and close-up around the tungsten oxide 002 peak

Figure 1. (a) Extended 2θ/ω2\theta/\omega scans of films deposited on sapphire with CO2\mathrm{CO}_2 for 30 min, 120 min, and without CO2\mathrm{CO}_2 (Ar). (b) Close-up around the tungsten oxide 002 peak

The 2θ/ω2\theta/\omega in Figure 1 and S1 showed a family of peak that is consistent with the {00l}\{00l\} planes of several phases of tungsten oxide, namely the monoclinic γ\gamma-WO3\mathrm{WO}_3, the orthorhombic β\beta-WO3\mathrm{WO}_3, the high-temperature monoclinic phase, and the tetragonal phase.[2] No reflections besides the ones of the substrate are observed when substituting CO2\mathrm{CO}_2 by Ar with a similar impurity level. Indicating that CO2\mathrm{CO}_2 is the main oxidizing species in the process. The asymmetry of the peak is similar to the one reported by other authors for γ\gamma-WO3\mathrm{WO}_3[14] and tetragonal WO3\mathrm{WO}_3[8] on r-cut sapphire and may originate from the relaxation of the film.

To get more insight into the symmetry of the phase, GID patterns and pole figures were recorded. The azimuth angle φ\varphi was set to zero for the scan aligned with the α\alpha-Al2_2O3_3[110] (or α\alpha-Al2_2O3_3[2 1\bar{1}0]) direction. GID scans were recorded for φ=0\varphi= 0, 4545, 9090 and 135∘135^\circ (Figure 2), forming two sets of orthogonal scans and for Ψ=89.5∘\Psi= 89.5^\circ, therefore corresponding to a 0.5∘0.5^\circ plane of incidence (assuming the sample perfectly flat). Only the {hk0}\{hk0\} families of planes (with hh or kk non-zero) are observed. This confirms the out-of-plane relationship as

GID patterns of the 120 min-deposited sample

Figure 2. GID patterns of the 120 min-deposited sample taken along the [110] direction of sapphire, and rotated by φ=45∘\varphi= 45^\circ, 90∘90^\circ and 135∘135^\circ and Ψ=89.5∘\Psi= 89.5^\circ. Low intensity, non-indexed peaks and shoulders match with Kβ radiation.

WO3(001)//α-Al2O3(011ˉ2).\mathrm{WO}_3(001) // \alpha\text{-}\mathrm{Al}_2\mathrm{O}_3(01\bar{1}2).

At φ=0∘\varphi= 0^\circ and φ=90∘\varphi= 90^\circ, only the {hk0}\{hk0\} plane families such as h=kh = k (e.g. {220}\{220\}) are found, from which we deduce the in-plane relationship to

WO3(110)//α-Al2O3(112ˉ0).\mathrm{WO}_3(110) // \alpha\text{-}\mathrm{Al}_2\mathrm{O}_3(11\bar{2}0).

These epitaxial relationships are the same as those reported for monoclinic or orthorhombic WO3\mathrm{WO_3} synthesized with other methods[7, 14, 16] and unlike reported in[8, 21] where {00l}\{00l\} is also found in-plane.

Even the ‘forbidden’ diffraction peaks from the {330}\{330\} and {550}\{550\} families of planes are detected. The presence of both {h00}\{h00\} and {0k0}\{0k0\} with similar intensities for both ϕ=45∘\phi= 45^\circ and 135∘135^\circ excludes the formation of high symmetry phases such as cubic and tetragonal WO3\mathrm{WO_3} while indicating a 90∘90^\circ rotational twinning. Distinguishing between orthorhombic β\beta- WO3\mathrm{WO_3} (Pbcn) and monoclinic γ\gamma- WO3\mathrm{WO_3} (P21_1/n) is known to be problematic.[7, 16] The h00h00 and 0k00k0 peak positions match better with the orthorhombic phase than the monoclinic one, one may argue that the influence of the substrate may affect in-plane interplanar distances.

XRD pole figures taken at 2θ=35.68∘2\theta= 35.68^\circ (Figure 3) confirm the epitaxial and twinned nature of the films. The poles in Figure 3 are distributed as follow: two sharp and weak poles at Ψ=44.9∘\Psi= 44.9^\circ, two sharp and intense poles at Ψ=47.7∘\Psi= 47.7^\circ, eight poles at Ψ=50.0∘\Psi= 50.0^\circ and four broad and weak poles at Ψ=72.2∘\Psi= 72.2^\circ. The sharp poles correspond to Al2O3{101ˉ4}\mathrm{Al_2O_3}\{10\bar{1}4\} (2θ=35.1512\theta= 35.151, Ψ=47∘\Psi= 47^\circ) and the tail of Al2O3{112ˉ0}\mathrm{Al_2O_3}\{11\bar{2}0\} (2θ=37.785∘2\theta= 37.785^\circ, Ψ=43∘\Psi= 43^\circ). The eight poles at Ψ=50.0∘\Psi= 50.0^\circ corresponds to WO3\mathrm{WO_3}, however, this can be interpreted either as the 122 poles of the orthorhombic phase, which appears as eight due to 90∘90^\circ rotational twinning (2×42 \times4 poles, the 212 reflections being extinct) or as the superposition of the 122, 1ˉ22\bar{1}22, 212 and 21ˉ22\bar{1}2 poles of the monoclinic phase, also resulting in eight poles. The monoclinic case would originate from four rotational twins due to its lower symmetry, however the broadening cause by the superposition is in the order of 1 to 2 degrees, which is lower than the step size of the measurement. Similarly, the poles at Ψ=72.2∘\Psi= 72.2^\circ are associated either to the 221 poles of the orthorhombic phase or the overlap of the 221 and 221‾\overline{221} poles of the monoclinic phase.

Pole figures recorded at $2\theta = 35.68^\circ$

Figure 3. Pole figures recorded at 2θ=35.68∘2\theta= 35.68^\circ. The three set of circles correspond three groups of poles.

The real part of the complex dielectric function ε1\varepsilon_1 obtained from VASE shows an increase from 5.15 at 1 eV to a maximum of about ≈13.3\approx13.3 at 4 eV (Figure 4). This matches well the one reported in a recent study[37] (ε1\varepsilon_1 rising from 6 and reaching a maximum of 12 at 4 eV). The imaginary part of the dielectric function ε2\varepsilon_2 and the absorption coefficient are low across most of the visible spectrum (with ε2<10−3\varepsilon_2 < 10^{-3}). between 1.7 and 2.6 eV) up to around 3 eV where a sharp increase in absorption is observed. The latter value is consistent with reported value of 2.9 eV for the indirect band gap of stoichiometric WO3\mathrm{WO}_3.[38]

Optical properties of a 30-nm WO3 thin film: real part of the dielectric function, imaginary part of the dielectric function, and absorption coefficient

Figure 4. Optical properties of a 30-nm WO3_3 thin film deposited on r-cut sapphire a) real part of the dielectric function, b) imaginary part of the dielectric function, and c) absorption coefficient. The feature at 4.5 eV is a fitting artifact.

Conclusion

We have demonstrated the epitaxial growth of monoclinic or orthorhombic WO3\mathrm{WO}_3 on r-cut sapphire by HFMOD using CO2\mathrm{CO}_2 as a precursor. The out-of-plane epitaxial relationship were WO3(001)//α-Al2O3(01ˉ12)\mathrm{WO}_3(001)//\alpha\text{-}\mathrm{Al}_2\mathrm{O}_3(0\bar{1}12) and the in-plane epitaxial relationships were either WO3(110)//α-Al2O3(11ˉ20)\mathrm{WO}_3(110)//\alpha\text{-}\mathrm{Al}_2\mathrm{O}_3(1\bar{1}20) or WO3(1ˉ10)//α-Al2O3(11ˉ20)\mathrm{WO}_3(\bar{1}10)//\alpha\text{-}\mathrm{Al}_2\mathrm{O}_3(1\bar{1}20) due to 90°-rotational twining. The optical properties, obtained from spectroscopic ellipsometry measurements, were consistent with stoichiometric WO3\mathrm{WO}_3.

Acknowledgments

We acknowledge funding from the Swedish Research Council VR under project no. 2025-03680, the Swedish Energy Agency under project no. P2025-03108, and the Knut and Alice Wallenberg foundation through the Wallenberg Academy Fellows program (KAW-2020.0196). We acknowledge Myfab Uppsala. Myfab is funded by the Swedish Research Council (2020-00207) as a national research infrastructure.

References

  1. [1]Wriedt, H. A. The O-W (oxygen-tungsten) system. Bull. Alloy Phase Diagrams 10, 368–384 (1989).DOI
  2. [2]Howard, C. J., Luca, V. & Knight, K. S. High-temperature phase transitions in tungsten trioxide - the last word ? High-temperature phase transitions in tungsten trioxide — the last word ? J. Phys. Condens. Matter 14, 377 (2002).
  3. [3]Goulding, M. R., Thomas, C. B. & HurdItch, R. J. A COMPARISON OF THERMO- AND PHOTO-CHROMIC BEHAVIOUR IN FILMS OF AMORPHOUS WO3. Solid State Commun. 46, 451–453 (1983).DOI
  4. [4]Yano, M. et al. Electrochromic properties of epitaxial WO3 thin films grown on sapphire substrates. Jpn. J. Appl. Phys. 57, (2018).DOI
  5. [5]Deb, S. K. A Novel Electrophotographic System. Appl. Opt. 8, 192–195 (1969).pubmed.ncbi.nlm.nih.gov/20076124
  6. [6]Bakhit, B. et al. Evidence for stabilization of ferroelectricity in WO3 thin films under anisotropic epitaxial strain. (2026) doi:10.1063/5.0317226.DOI
  7. [7]LeGore, L. J., Greenwood, O. D., Paulus, J. W., Frankel, D. J. & Lad, R. J. Controlled growth of WO3 films. J. Vac. Sci. Technol. A 15, 1223–1227 (1997).DOI
  8. [8]Moulzolf, S. C., LeGore, L. J. & Lad, R. J. Heteroepitaxial growth of tungsten oxide films on sapphire for chemical gas sensors. Thin Solid Films 400, 56–63 (2001).DOI
  9. [9]Mattinen, M. et al. Atomic Layer Deposition of Molybdenum and Tungsten Oxide Thin Films Using Heteroleptic Imido-Amidinato Precursors : Process Development , Film Characterization , and Gas Sensing Properties Atomic Layer Deposition of Molybdenum and Tungsten Oxide Thin Film. Chem. Mater. 30, 8690–8701 (2018).DOI
  10. [10]Cohen, A. et al. Tungsten Oxide Mediated Quasi-van der Waals Epitaxy of WS 2 on Sapphire. ACS Nano 17, 5399–5411 (2023).DOI
  11. [11]Díaz-Reyes, J.; Dorantes-García, V.; Pérez-Benítez, A.; Balderas-López, J. A. Obtaining of films of tungsten trioxide (WO3) by resistive heating of a tungsten filament. Superf. y vacío 21, 12–17 (2008).
  12. [12]Shankar, N., Yu, M., Vanka, S. P. & Glumac, N. G. Synthesis of tungsten oxide ( WO 3 ) nanorods using carbon nanotubes as templates by hot filament chemical vapor deposition. 60, 771–774 (2006).DOI
  13. [13]Kobayashi, Y., Terada, S. & Kubota, K. Epitaxial growth of WO3 thin films on MgO and Al2O3. Thin Solid Films 168, 133–139 (1989).DOI
  14. [14]A Garg, J., Leake, A. & Barber, Z. H. Epitaxial growth of WO 3 films on SrTiO 3 and sapphire. J. Phys. D Appl. Phys. 33, 1048 (2000).DOI
  15. [15]Leng, X., Pereiro, J., Strle, J., Bollinger, A. T. & Božović, I. Epitaxial growth of high quality WO3 thin films. APL Mater. 3, 1–6 (2015).DOI
  16. [16]Yano, M. et al. Growth and crystallographic characterization of molecular beam epitaxial WO 3 and MoO 3 /WO 3 thin films on sapphire substrates. Appl. Surf. Sci. 381, 32–35 (2015).
  17. [17]Thangala, J. et al. Large-Scale , Hot-Filament-Assisted Synthesis of Tungsten Oxide and Related Transition Metal Oxide Nanowires. 40292, 890–896 (2007).pubmed.ncbi.nlm.nih.gov/17415736
  18. [18]Lu, D., Liang, B., Ogino, A. & Nagatsu, M. Study of the synthesis of tungsten trioxide nanostructured arrays by tungsten hot filament chemical vapor deposition method and their field emission properties. AIP Adv. 1–7 (2010) doi:10.1116/1.3292599.DOI
  19. [19]Escalante, G. et al. Correlation between Raman spectra and color of tungsten trioxide (WO3 ) thermally evaporated from a tungsten filament. AIP Adv. 11, 055103 (2021).DOI
  20. [20]Houweling, Z. S. et al. Growth process conditions of tungsten oxide thin films using hot-wire chemical vapor deposition. Mater. Chem. Phys. 131, 375–386 (2011).DOI
  21. [21]Tägstöm, P. & Jansson, U. Chemical vapour deposition of epitaxial WO3 films. Thin Solid Films 352, 107–113 (1999).DOI
  22. [22]Dezelah, C. L. I. et al. Atomic Layer Deposition of Tungsten ( III ) Oxide Thin Films from W 2 ( NMe 2 ) 6 and Water : Precursor-Based Control of Oxidation State in the Thin Film Material. J. Am. Chem. Soc. Am. Chem. Soc. 128, 9638–9639 (2006).
  23. [23]Ito, A. & Morishita, Y. Selective self-oriented growth of (2 0 0), (0 0 2), and (0 2 0) d-WO3 films via metal-organic chemical vapor deposition. Mater. Lett. 258, 126817 (2020).DOI
  24. [24]Nishihaya, S. et al. Evolution of Insulator – Metal Phase Transitions in Epitaxial Tungsten Oxide Films during Electrolyte-Gating. Appl. Mater. Interfaces (2016) doi:10.1021/acsami.6b06593.DOI
  25. [25]Yang, J. et al. Effects of line defects on the electronic and optical properties of strain-engineered WO3 thin films. J. Mater. Chem. C 5, 11694–11699 (2017).DOI
  26. [26]Mattoni, G., Filipetti, A., Manca, N., Zubko, P. & Caviglia, A. D. Charge doping and large lattice expansion in oxygen-deficient heteroepitaxial WO 3. Phys. Rev. Mater. 2, 053402 (2018).DOI
  27. [27]Kellett, E. A. & Rogers, S. E. The Structure of Oxide Layers on Tungsten. J. Electrochem. Soc. 110, 502 (1963).DOI
  28. [28]Abel, W. T., Spencer, J. D. & Bailey, D. M. Hot Filament Method of Determining Oxidizing Gases in High-Purity Gas Streams. Anal. Chem. 37, 1711–1715 (1965).DOI
  29. [29]Warren, A. & Nylund, A. Oxidation of Tungsten and Tungsten Carbide in Dry and Humid Atmospheres. 14, 345–353 (1996).
  30. [30]Habainy, J., Iyengar, S., Babu, K. & Lee, Y. Formation of oxide layers on tungsten at low oxygen partial pressures. J. Nucl. Mater. 506, 26–34 (2018).DOI
  31. [31]Blackburn, B. P. E., Hoch, M. & Johnston, H. L. THE VAPORIZATION OF MOLYBDENUM AND TUNGSTEN OXIDES. J. Phys. Chem. 62, 769–773 (1958).
  32. [32]Harvey, F. J. High Temperature Oxidation of Tungsten Wires in CO2-Argon Mixtures. Metall. Trans. 5, 35–38 (1974).DOI
  33. [33]Shaffer, J. W. IMPROVED GETTER FOR INCANDESCENT LAMPS. 9 (1989).
  34. [34]Wang, L. U., Bu, C., Zhang, G. & Wang, J. Study of the Reduction of Industrial Grade MoO 3 Powders with CO or CO-CO 2 Gases to Prepare. Metall. Trans. B 48, 2047–2056 (2017).
  35. [35]Larrabee, R. D. Spectral Emissivity of Tungsten. J. Opt. Soc. Am. 49, 619–625 (1959).
  36. [36]Cezairliyan, A. & McClure, J. L. High-Speed ( Subsecond ) Measurement of Heat Capacity , Electrical Resistivity , and Thermal Radiation Properties of Tungsten in the Range 2000 to 3600 K *. J. Res. Notional Bur. Stand. - A. Phys. Chem. 75A, 283–290 (1971).DOI
  37. [37]Sekora, D., Mock, A., Korlacki, R., Echeverr, E. M. & Ianno, N. Critical-point model dielectric function analysis of WO 3 thin films deposited by atomic layer deposition techniques. 1–6.DOI
  38. [38]Iwai, T. Temperature Dependence of the Optical Absorption Edge of Tungsten Trioxide Single Crystal. J. Phys. Soc. Japan 15, 1596 (1960).DOI

Paper details

vlnc:W_3nv5tb9w
Version
v1 · latest
Published
Fresh — added to the Hub within the last 30 days
Added
License
CC BY 4.0
Usage

views · 0

downloads · 0

A view counts once per browser per day, a download each time the PDF is requested.

  • Physics and Astronomy