betaFeedback

WorksPhysics and Astronomy

An analysis on improvement of x-ray diffractometer results by controlling and calibration of parameters

Abstract

The X-ray diffractometer in the laboratory is a crucial instrument for analyzing materials in science. It can be used on almost any crystal material, and if the machine parameters are appropriately controlled, it can offer a lot of information about the samples characteristics. Nevertheless, the data obtained from these machines are complicated by an aberration function that can be resolved through calibration. In this study, a powder comprising of Barium Sulfate (BaSO4), Zinc Oxide (ZnO) and Aluminum (Al) was used as the first sample and a single crystal sample comprised of Gallium Nitride (GaN) and Aluminum Oxide (Al2O3). The required calibration parameters of the X-ray diffractometer namely: Straight Beam Alignment, Beam Cut Alignment and Sample Tilt Alignment for two samples were analyzed and carried out. Using the results of the X-ray spectrum, important parameters such as corresponding planes for peak positions, d-spacing of planes, intensities, smallest crystallite sizes and lattice parameters, and a comparison with the reference data were all carried out. As another result, the out-of-plane alignment and Full-Width at Half-Maximum (FWHM) value for GaN could be determined using the rocking curve.

Introduction

The X-ray powder diffractometer, a versatile analytical instrument employed in various scientific disciplines, including material science [1, 2, 3, 4], geology [5], and biomedical device analysis [6, 7, 8], plays a crucial role in characterizing crystalline materials. It can collect a continuous suite of hkl reflections with a single scan in θ\theta-2θ2\theta angle space and is suitable for small crystallites ranging from 55 μm\mu\text{m} to 3030 μm\mu\text{m}. With advanced data analysis methods, it can provide both qualitative and quantitative information [9, 10]. Modern commercial instruments may have additional features like focusing mirror optics and interchangeable experimental configurations.

On the one hand, conducting numerical analysis requires statistical analysis [11, 12, 13, 14] [15] and experimental design, susceptible to errors and barriers such as uncertainty [16]. On the other hand, every experimental work needs a good calibration and inspection [17–20]. The divergent beam X-ray diffractometer can illuminate many crystallites, resulting in a strong diffraction signal from a representative portion of the sample. However, the para-focusing optics of laboratory diffractometers produce complex profile shapes that do not necessarily reflect the proper spacing of hkl planes. Modeling these aberrations requires further analysis, but there are also instrumental effects that are not well understood and can lead to confounding results when instruments are set up incorrectly. Therefore, the use of SRMs to calibrate instrument performance is preferred to avoid these situations.

BaSO4\mathrm{BaSO}_{4} powders are commonly used in coatings for the internal surfaces of spectrophotometers integrating spheres, construction materials, and household paints. These coatings are characterized by their diffuse reflection spectrum and integral absorption coefficient of solar radiation [21,22]. BaSO4\mathrm{BaSO}_{4} powders have a high reflectance in the UV, visible, and near IR regions of the spectrum [23–25], making them ideal for reflective coatings in spectrophotometers. The approximate band gap of BaSO4\mathrm{BaSO}_{4} is 6 eV, with the main absorption edge at around 200 nm [26]. In contrast, coatings based on ZnO\mathrm{ZnO} and TiO2\mathrm{TiO}_{2} powders exhibit significantly larger solar absorptivity values, ranging from 0.15 to 0.19 for ZnO\mathrm{ZnO} pigment-based coatings and 0.17 to 0.2 for TiO2\mathrm{TiO}_{2} pigment-based coatings [27]. The coefficient αs\alpha_{\mathrm{s}} of white pigments in ZnO\mathrm{ZnO} used in coatings typically ranges from 0.15 to 0.2 [28,29], while titanium dioxide powder-based coatings have a coefficient that can reach up to approximately 0.28 [29].

The absorption coefficient αs\alpha_{\mathrm{s}} can be reduced by increasing the reflection coefficient ρ\rho of the powders in longer wavelength regions than the main absorption edge of the solar spectrum. The size of powder particles and impurities in the powder pigment also affect ρ\rho in different spectrum regions.

For a powder to have a high ρ\rho value across a broad spectrum, such as the solar one (0.2–3.0 μm\mu\mathrm{m}), it must be very pure and have particles that closely match this spectrum [30]. Adding nanoparticles is one way to alter how big the powder particles are and prevent them from losing their optical qualities when exposed to space radiation [31,32]. This helps achieve the maximum increase in their stability under radiation [33].

Some nanopowders that can modify pigments are ZnO\mathrm{ZnO}, ZrO2\mathrm{ZrO}_{2}, Al, etc. [34]. However, the optical qualities of BaSO4\mathrm{BaSO}_{4} powders and other substances that are modified by these nanopowders may change differently. The modification may only improve their reflectivity a little. That is why such research is scientifically and practically relevant. This study focuses on the first sample, which consists of BaSO4\mathrm{BaSO}_{4}, ZnO\mathrm{ZnO} and Al.

Some insulators like SiO2\mathrm{SiO}_{2}, SiNx\mathrm{SiN}_{x}, Al2O3\mathrm{Al}_{2}\mathrm{O}_{3}, and HfO2\mathrm{HfO}_{2} can help reduce gate current and protect the surface of GaN metal insulator semiconductor high electron mobility transistors (MISHMETs) [35–37]. Al2O3\mathrm{Al}_{2}\mathrm{O}_{3} has some advantages, such as a big band gap, breakdown electric field, and simple deposition. The dielectric/GaN interface is crucial for how well GaN-based MISHMETs perform for mm-wave and power switching uses.

The main desire in this work is to determine sources of measurement error and the procedures to calibrate the laboratory X-ray diffraction instrument properly. In this regard, first, the required alignments for the machine were carried out: Straight Beam Alignment, Beam Cut Alignment and Sample Tilt Alignment for the diffractometer. After conducting the X-ray diffraction, we could match the materials used in both samples, the powder comprised of BaSO4\mathrm{BaSO}_{4}, ZnO\mathrm{ZnO} and Al and the single crystal sample comprised of GaN and Al2O3\mathrm{Al}_{2}\mathrm{O}_{3}. The corresponding planes for peak positions, intensities, comparison with the reference data, the smallest crystallite sizes and lattice parameters were all carried out using the results of the X-ray spectrum. The rocking curve of the GaN also helped find the out-of-plane alignment and Full-Width-at Half-Maximum (FWHM) value. Notably, this work significantly contributes to the field by providing comprehensive insights and practical guidance on the calibration and alignment of X-ray diffractometers, facilitating accurate material analysis and advancing scientific research quality, making it a valuable addition to the academic literature.

Materials and Methods

In this experiment, using X-ray diffraction, a Panalytical X’Pert PRO X-ray diffractometer matches the crystal structure and phases of two samples (powder and single crystal) using X-ray diffraction. In the first step, a radiation measurement will be conducted using a Geiger counter to ensure the safety of the experiment. A Cu radiation with Kα1\mathrm{K}\alpha_{1} wave length of 1.5406Å was used in this experiment. The voltage and current of the generator were set to be 45 KV and 40 mA, respectively.

Loading sample and beam optics hardware

For the first sample, which is comprised of BaSO4\mathrm{BaSO}_{4}, ZnO\mathrm{ZnO} and Al, at the incident side of the experiment, a 1/321/32 divergence slit to control the intensity of the diffracted beam and a Cu (0.2 mm)/Ni (0.02 mm) attenuator to reduce the incident beam intensity by a specific factor, are used. The smallest possible divergence slit is used to prevent any deviation in the X-ray beam at low incident angles. At the receiving side, a 0.27° receiving slit and a 0.04 rad soller slit for collimation of diffracted beam and enhancing the resolution of the scans, are used. Notably, Ni in the attenuator performs as a filter for the KβK\beta line. It features the maximum possible KαK\alpha line while reducing the intensity of the KβK\beta line. On the other hand, Cu does not absorb any radiation, yet it scatters it.

For the other sample (Fig.1), which is comprised of GaN and Al2O3Al_2O_3, first, a 1/2∘1/2^\circ divergence slit with Ni 0.02 filter is used. Type 0.27° and 0.04 rad soller slit collimators are used on the receiving side of the machine. Besides mentioned, an automatic 0.125 mm Ni beam attenuator helps in automatic insertion/removal of the attenuator.

Image not extracted

Figure 1. Thin film sample

Beam alignment for a powder sample

Straight beam alignment In this step, the 2θ2\theta angle is aligned at the 0 position of the straight beam. An I-2θ2\theta plot is derived to fulfill the alignment (Fig.2).

Image not extracted

Figure 2. Straight Beam Alignment

Beam Cut Alignment This process, also known as Z alignment, aligns the sample’s surface to the diffractometer’s center (Fig.3). In this Step, an I-Z plot is generated.

Image not extracted

Figure 3. Beam Cut Alignment

Sample Tilt Alignment This procedure, which is also known as ω\omega alignment, is performed to make the sample surface parallel to the straight beam as depicted in Fig. 4. Notably, in our case ω=θ\omega= \theta.

Image not extracted

Figure 4. Tilt Alignment

After the alignment, a full θ\theta-2θ2\theta scan in the range of (20°-80°) and with 0.02 scan step size will be conducted to determine the peak positions and relative intensities of X-ray diffraction.

RESULTS AND DISCUSSION

In this section, the X-ray spectrum of both samples will be illustrated and indexed using reference data from the International Center for Diffraction Data (ICDD). In the next step, a comparison between experimental and ICDD data for intensities has been illustrated, as well as plane spacing. Besides, the smallest crystallite size of each component is calculated.

Powder sample

Fig. 5 shows θ\theta-2θ2\theta full scan spectrum of X-ray diffraction as well as the index of each plane based on ICDD data for all components namely BaSO4BaSO_4, ZnO and Al [38].

Table 1 shows the angle and intensity of peak positions in both experimental data and the ICDD file. Also, the d-spacing of planes for each material component can be seen. From Table 1 we can see that the 2θ2\theta difference between experimental and reference data is almost constant for each material component at different angles. We see two changes for BaSO4BaSO_4 from the reference at 1-2 and 4-5 peaks, and for Al in 1-2 peak. All the discrepancies in the spectrum could be because of thermal, residual strain, preferred orientation, and production factors [39]. As shown in Table 1 there are fewer peaks for Al and ZnO which could be due to a lower content of these components in the powder sample.

Based on the ICDD files, we know that the crystal structure for BaSO4_4, ZnO and Al are orthorhombic, hexagonal and cubic, respectively. Therefore, we can find the corresponding crystal parameters illustrated in Table 2.

MaterialFormulaa(Å)b(Å)c(Å)
ZnO1d2=43(h2+hk+l2a2)+l2c2\frac{1}{d^2}=\frac{4}{3}\left(\frac{h^2+hk+l^2}{a^2}\right)+\frac{l^2}{c^2}3.243.245.2
BaSO4_41d2=h2a2+k2b2+l2c2\frac{1}{d^2}=\frac{h^2}{a^2}+\frac{k^2}{b^2}+\frac{l^2}{c^2}7.088.775.46
Aldhkl=ah2+k2+l2d_{hkl}=\frac{a}{\sqrt{h^2+k^2+l^2}}4.054.054.05

Table 2. Lattice Parameters for a powder diffraction

Table 3 illustrates the smallest crystallite size for the powder sample using the Scherrer equation [40] as Eq. (1):

t=0.9λBcos⁡θB(1)t = \frac{0.9\lambda}{B\cos\theta_B} \tag*{(1)}

For ZnO, BaSO4_4 and Al, the highest intensities were found at 2θ2\theta angles of 36.23°, 42.57° and 44.59°, respectively. Therefore, these peaks were used to determine the crystallite sizes in Table 3.

Materialhkl planeRelative Intensityθ\theta (°)B (Rad)×10−3\times10^{-3}t (nm)
ZnO10110018.124.5432.13
BaSO4_414081.3321.294.1935.51
Al20062.2222.304.8930.65

Table 3. Smallest crystallite size of a powder sample

Experimental 2θ2\theta (°)Real IntensityRelative IntensityICDD 2θ2\theta (°)ICDD Relative Intensity2θ2\theta Differenced (Å)=λ/2sinθMaterialhkl plane
22.797131.5622.81500.033.89BaSO4_4111
24.86723224.89300.033.57BaSO4_4200
25.8113660.4425.861000.053.44BaSO4_4021
26.8117879.1126.86700.053.32BaSO4_4210
28.7116874.6728.77950.063.10BaSO4_4121
31.5511048.8931.555002.83BaSO4_4211
31.7312957.3331.80570.072.81ZnO100
32.775825.7832.82450.052.73BaSO4_4002
34.417834.6734.45440.042.60ZnO002
36.2322510036.281000.052.47ZnO101
38.313716.4438.501000.192.34Al111
40.793816.8940.81250.022.21BaSO4_4122
42.5718381.3342.63800.062.12BaSO4_4140
42.9114062.2242.95750.042.10BaSO4_4212
43.994921.7844.02190.032.05BaSO4_4041
44.5914062.2244.78470.192.03Al200
47.53452047.58230.051.91ZnO102
48.995122.6749.04180.051.85BaSO4_4330
56.617432.8956.65320.051.62ZnO110
62.836127.1162.92290.091.47ZnO103
65.075323.5665.19220.121.43Al220
67.915524.4468.02230.111.37ZnO112
78.116629.3378.30240.191.22Al311

Table 1. Powder sample crystal planes comparison with the ICDD data

Image not extracted

Figure 5. X-ray spectrum for a powder sample

Thin film sample

Figure 6 shows θ\theta-2θ2\theta full scan spectrum of X-ray diffraction and the index of each plane based on the ICDD data for a single crystal sample with GaN and Al2_2O3_3 [38] components. It can be seen that just a family of planes that are parallel to (100) are illustrated. It is because of the preferred orientation effect. All other planes not parallel to (100) will be canceled from the plot.

Image not extracted

Figure 6. X-ray spectrum for thin film sample

Table 4 shows the angle and intensity of peak positions in both experimental data and the ICDD file for a single crystal sample. The d-spacing of planes for each material component can be seen, too. The results show a high difference between the film intensity (GaN) and substrate (Al2_2O3_3) which can be due to the beam bisection alignment method used while performing the experiment.

For GaN, Al2_2O3_3, the highest intensities were found at 2θ2\theta angles of 34.51° and 41.61°, respectively. Therefore, these peaks were used to determine the crystallite sizes in Table 5.

Based on the ICDD files, we know that the crystal structures for GaN and Al2_2O3_3 are hexagonal and Rhombohedral, respectively. Therefore, we can find the corresponding crystal parameters illustrated in Table 6.

In Figure 7 the ω\omega-scan for GaN, which is also called a rocking curve for the sample, can be seen. We can also see the peak center and Full-Width-at Half-Maximum (FWHM) inside the plot.

Image not extracted

Figure 7. Rocking curve of GaN

In the Figure 7, the peak center is at 17.232°; however the data shows that the peak center is at ½ ×\times 34.59 = 17.295. Therefore, there is 0.063° which can be because of several reasons, such as residual stress in the film. A low amount of FWHM shows that the crystallinity of the sample is good.

Experimental 2θ2\theta (°)Real IntensityRelative IntensityICDD 2θ2\theta (°)ICDD Relative Intensity2θ2\theta Differencedd (Å)=λ/2sin⁡θ\lambda/2\sin\thetaMaterialhkl plane
34.51613871110034.59450.082.59GaN002
41.61583590.9541.7150.12.16Al2_2O3_3006
72.855423458.8372.9830.131.29GaN004

Table 4. Thin film crystal planes comparison with the ICDD data

Materialhkl planeRelative Intensityθ\theta (°)B (Rad)×10−3^{-3}t (nm)
GaN00210017.253.1446.23
Al2_2O3_30060.9520.814.8930.33

Table 5. Smallest crystallite size of thin film sample

MaterialFormulaa(Å)b(Å)c(Å)
GaN1d2=43(h2+hk+l2a2)+l2c2\frac{1}{d^2}=\frac{4}{3}\left(\frac{h^2+hk+l^2}{a^2}\right)+\frac{l^2}{c^2}UnknownUnknown5.18
Al2_2O3_31d2=1a2(1+cos⁡α){(h2+k2+l2)−(1−tan⁡212α)(hk+kl+lh)}c1+cos⁡α−2cos⁡2α\frac{1}{d^2}=\frac{1}{a^2}\frac{(1+\cos\alpha)\{(h^2+k^2+l^2)-(1-\tan^2\frac{1}{2}\alpha)(hk+kl+lh)\}c}{1+\cos\alpha-2\cos^2\alpha}UnknownUnknownUnknown

Table 6. Lattice Parameters for single crystal sample

Conclusions

In summary, this work represents a crucial step forward in the field of materials science and instrumentation by meticulously investigating the sources of measurement error in X-ray diffraction experiments and implementing effective calibration procedures. For this purpose, 2 X-ray diffraction analyses were conducted on two different samples of powder and single crystal materials, namely: a powder comprised of BaSO4_4, ZnO and Al, as the first sample, and a single crystal sample comprised of GaN and Al2_2O3_3. Considering the results, indexing all the peak positions in the θ\theta-2θ2\theta scan was carried out, and the important parameters like d-spacing of planes, smallest crystallite sizes, crystal structures and lattice parameters were also determined. The rocking curve of the single crystal film determined the out-of-plane alignment and FWHM value. By ensuring the accuracy and reliability of X-ray diffraction data, this work underpins the foundation of scientific research in materials characterization and instrumentation, ultimately advancing our knowledge and contributing to the robustness of scientific outcomes.

References

  1. [1]J.V. Bernier, R.M. Suter, A.D. Rollett, J.D. Almer, High-Energy X-Ray Diffraction Microscopy in Materials Science. Annual Review of Materials Research, 50, 2020: 395-436. https://doi.org/10.1146/annurev-matsci-070616-124125
  2. [2]A. Pandey, S. Dalal, S. Dutta, A. Dixit, Structural characterization of polycrystalline thin films by X-ray diffraction techniques. Journal of Materials Science: Materials in Electronics, 32, 2021: 1341-1368. https://doi.org/10.1007/s10854-020-04998-w
  3. [3]M. Kashi, F. Baghbani, F. Moztarzadeh, H. Mobasheri, E. Kowsari, Green synthesis of degradable conductive thermosensitive oligopyrrole/chitosan hydrogel intended for cartilage tissue engineering. International Journal of Biological Macromolecules, 107(Part B), 2018: 1657-1755. https://doi.org/10.1016/j.ijbiomac.2017.10.015
  4. [4]F. Baghbani, F. Moztarzadeh, M. Mozafari, M. Raz, H. Rezvani, Production and Characterization of a Ag- and Zn-Doped Glass-Ceramic Material and In Vitro Evaluation of Its Biological Effects. Journal of Materials Engineering and Performance, 25, 2016: 3398-3408. https://doi.org/10.1007/s11665-016-2156-7
  5. [5]E.B. Rampe, D.F. Blake, T.F. Bristow, D.W. Ming, D.T. Vaniman, et al., Mineralogy and geochemistry of sedimentary rocks and eolian sediments in Gale crater, Mars: A review after six Earth years of exploration with Curiosity. Geochemistry, 80(2), 2020: 125605. https://doi.org/10.1016/j.chemer.2020.125605
  6. [6]A.H. Foroughi, C. Valeri, D. Jiang, F. Ning, M. Razavi, M.J. Razavi, Understanding compressive viscoelastic properties of additively manufactured PLA for bone-mimetic scaffold design. Medical Engineering & Physics, 114, 2023: 103972. https://doi.org/10.1016/j.medengphy.2023.103972
  7. [7]M.M. Quazi, M. Ishak, M.A. Fazal, A. Arslan, S. Rubaiee, et al., A comprehensive assessment of laser welding of biomedical devices and implant materials: recent research, development and applications. Critical Reviews in Solid State and Materials Sciences, 46(2), 2021: 109-151. https://doi.org/10.1080/10408436.2019.1708701
  8. [8]M. Shahrezaee, M. Raz, S. Shishehbor, F. Moztarzadeh, F. Baghbani, A. Sadeghi, et al., Synthesis of Magnesium Doped Amorphous Calcium Phosphate as a Bioceramic for Biomedical Application: In Vitro Study. Silicon, 10, 2018: 1171-1179. https://doi.org/10.1007/s12633-017-9589-y
  9. [9]F. Baghbani, F. Moztarzadeh, L. Hajibaki, M. Mozafari, Synthesis, characterization and evaluation of bioactivity and antibacterial activity of quinary glass system (SiO₂–CaO–P₂O₅–MgO–ZnO): In vitro study. Bulletin of Materials Science, 36, 2013: 1339-1346. https://doi.org/10.1007/s12034-013-0593-6
  10. [10]Sh.S. Seyedmomeni, M. Naeimi, M. Raz, J.A. Mohandesi, F. Moztarzadeh, F. Baghbani, M. Tahiri, Synthesis, Characterization and Biological Evaluation of a New Sol-Gel Derived B and Zn-Containing Bioactive Glass: In Vitro Study. Silicon, 10, 2018: 197-203. https://doi.org/10.1007/s12633-016-9414-z
  11. [11]H. Moradi, R.B, Aein, G. Youssef, Multi-objective design optimization of dental implant geometrical parameters. International Journal for Numerical Methods in Biomedical Engineering, 37(9), 2021: e3511. https://doi.org/10.1002/cnm.3511
  12. [12]M. Noorbakhsh, H.R. Moradi, Design and optimization of multi-stage manufacturing process of stirling engine crankshaft. SN Applied Sciences, 2, 2019: 65. https://doi.org/10.1007/s42452-019-1820-6
  13. [13]M.A. Khuda, J. Khalesi, Z. Tu, Y. Long, D.P. Koch, N. Sarunac, Numerical analysis of a developing turbulent flow and conjugate heat transfer for molten salt and liquid sodium in a solar receiver. Applied Thermal Engineering, 217, 2022: 119156. https://doi.org/10.1016/j.applthermaleng.2022.119156
  14. [14]S.B. Ferdosi, M. Porbashiri, Calculation of the Single-Walled Carbon Nanotubes’ Elastic Modulus by Using the AsymptoticDOI

Paper details

vlnc:W_4zden2ep
Version
v1 · latest
Published
Fresh — added to the Hub within the last 30 days
Added
License
CC BY 4.0
Usage

views · 0

downloads · 0

A view counts once per browser per day, a download each time the PDF is requested.

  • Physics and Astronomy

Not recorded for this paper

View statement
Looking for related papers…
Contents