betaFeedback

WorksPhysics and Astronomy

Revealing the ultra-fast domain wall motion in Manganese Gold through permalloy capping

Abstract

Antiferromagnets offer much faster dynamics compared to their ferromagnetic counterparts but their order parameter is extremely difficult to detect and control. So far, controlling the Néel order parameter electrically is limited to only very few materials where Néel spin-orbit torques are allowed by symmetry. In this work, we show that coupling a thin ferromagnet (permalloy) layer on top of an antiferromagnet (Mn2_2Au) solves a major roadblock – the controlled reading, writing, and manipulation of antiferromagnetic domains. We confirm by atomistic spin dynamics simulations that the domain wall patterns in the Mn2_2Au are imprinted on the permalloy, therefore allowing for indirect imaging of the Néel order parameter. Our simulations show that the coupled domain wall structures in Mn2_2Au-Py bilayers can be manipulated by either acting on the Néel order parameter via Néel spin-orbit torques or by acting on the magnetisation (the ferromagnetic order parameter) via magnetic fields. In both cases, we predict ultra-high domain wall speeds on the order of 8.5 km/s. Thus, employing a thin ferromagnetic layer has the potential to easily control the Néel order parameter in antiferromagnets even where Néel spin-orbit torques are forbidden by symmetry. The controlled manipulation of the antiferromagnetic order parameter provides a promising basis for the development of high-density storage and efficient computing technologies working in the THz regime.

Introduction

Spintronics has revolutionised data storage technology with spin current-based technologies such as hard disk drives. However, these devices are reaching the limit of possible technological advances in speed and size due to the intrinsic limits of ferromagnetic (FM) materials. In these devices, antiferromagnetic (AFM) materials are typically only used to provide a preferred direction of magnetisation for the active FM components. Using AFMs instead of FMs as the active component could solve this problem due to their ultra-fast dynamics, lack of external magnetic fields, and temperature stability of the Néel ordered state [4, 5, 6, 7] [1, 2, 3]. This brings massive advancements towards ultrafast and ultra high-density spintronics.

One of the most promising materials for AFM spintronic-based devices is manganese gold (Mn2Au\mathrm{Mn}_2\mathrm{Au}) due to its high Néel temperature, moderate anisotropy, and layered two-sublattice spin structure. It has been predicted that in certain AFMs current-induced spin-orbit-torques (SOTs) can switch the sub-lattice magnetic orientation [1, 2]. Recently these so-called Néel SOTs have been demonstrated experimentally for CuMnAs [8, 9, 10, 11] and Mn2Au\mathrm{Mn}_2\mathrm{Au} [12, 13] and materials with similar AFM ordering [14, 15, 16, 17]. However, detecting the AFM magnetic signal is far more difficult due to the absence of a net magnetisation.

Recently, a strong exchange coupling between Mn2Au\mathrm{Mn}_2\mathrm{Au} and thin layers of permalloy (Ni80Fe20\mathrm{Ni}_{80}\mathrm{Fe}_{20}) has been observed [18, 19]. As a consequence, the FM domain structure exactly maps the AFM domain structure [4, 18]. Notably, the coercive field of Mn2Au\mathrm{Mn}_2\mathrm{Au}-Py is an order of magnitude higher (5000 Oe [18]) compared to other materials such as CuMnAs (∼200\sim200 Oe [20]). High coercive fields lead to long-term stability at room temperature.

Due to the strong coupling, it is anticipated that the AFM Néel vector and the FM magnetisation rotate coherently when an external field is applied to the FM. While experimentally

the ultrafast dynamics (∝\propto THz) and current induced Néel SOT switching have yet to be demonstrated in Mn2Au\mathrm{Mn}_2\mathrm{Au}-Py, this report aims to showcase the promising prospects of Mn2Au\mathrm{Mn}_2\mathrm{Au}-Py bilayers. Atomistic simulations are used to accurately re-semble realistic crystal structures and material parameters in dynamics simulations. We derive a phenomenological model which is in agreement with the simulation results. Besides single domain states of the Mn2Au\mathrm{Mn}_2\mathrm{Au}-Py bilayer system, we simulate the driven dynamics of a domain wall percolating the FM/AFM bilayer by i) an applied magnetic field and ii) Néel SOTs. In both cases, we observe a strongly coupled domain wall motion with domain wall speeds on the order of 8.5 km/s.

Model of Mn2Au-Py bilayers

Here, we model a Mn2_2Au-Py bilayer system containing a 90-degree domain wall along the [100] direction which is capped by a thin layer of Py. The domain wall from the Mn2_2Au permeates through to the permalloy due to the strong interface coupling as shown in Figure 1 (a). The crystal structures of permalloy and Mn2_2Au are shown in Figure 1 (b) and (c) respectively. Although py is amorphous in bulk, due to interface lattice matching with the Mn2_2Au we presume that Py will have a BCC structure in the thin films we are simulating. The lattice structure of Mn2_2Au has two AFM coupled planes of Mn atoms and a plane of gold atoms. The Hamiltonian H\mathcal{H} of the Mn2_2Au-Py bilayer is comprised of three contributions:

Schematic diagram of a 90-degree magnetic domain wall in a Mn2Au-Py bilayer

Figure 1. (a) Schematic diagram of a 90-degree magnetic domain wall in a Mn2Au\mathrm{Mn}_2\mathrm{Au}-Py bilayer. The Mn2Au\mathrm{Mn}_2\mathrm{Au} layer is shown in blue and is capped by permalloy shown in grey. (b) and (c) detail the magnetic structures of permalloy and Mn2Au\mathrm{Mn}_2\mathrm{Au}, respectively.

H=HMn2Au+HPy+Hint,(1)\mathcal{H}=\mathcal{H}_{\mathrm{Mn_2Au}}+\mathcal{H}_{\mathrm{Py}}+\mathcal{H}_{\mathrm{int}}, \tag*{(1)}

the Hamiltonian describing Mn2_2Au (HMn2Au\mathcal{H}_{\mathrm{Mn_2Au}}), the Hamiltonian for permalloy (HPy\mathcal{H}_{\mathrm{Py}}), and the Hamiltonian for the interface (Hint\mathcal{H}_{\mathrm{int}}).

The Hamiltonian for Mn2_2Au up to the fourth order in anisotropy is given by [21]

HMn2Au=−∑i<j(SiJijMn2AuSj+SizJijMn2AuSjz)+∑i(k4(Siz)4+kϕ(Six)2(Siy)2)+Hd,(2)\mathcal{H}_{\mathrm{Mn_2Au}}=-\sum_{i<j}\left(\mathbf{S}_{i}\mathbf{J}^{\mathrm{Mn_2Au}}_{ij}\mathbf{S}_{j}+S_{i}^{z}J^{\mathrm{Mn_2Au}}_{ij}S_{j}^{z}\right)+\sum_{i}\left(k_{4}(S_{i}^{z})^{4}+k_{\phi}(S_{i}^{x})^{2}(S_{i}^{y})^{2}\right)+\mathcal{H}_{d}, \tag*{(2)}

where Si,j\mathbf{S}_{i,j} are unit vectors describing the local spin directions on sites i,ji,j. The first term describes the exchange energy, which incorporates the second order two-ion anisotropy [22]. The second term describes the fourth-order anisotropy, and Hd\mathcal{H}_{d} represents the magnetostatic fields. The dominant anisotropy in Mn2_2Au is the second order easy plane anisotropy. The weaker fourth-order anisotropy terms create easy axis anisotropy directions along the zz direction, i.e. k4<0k_{4}<0 as well as a term that breaks the in-plane rotational symmetry favouring the four symmetry equivalent ⟨110⟩\langle110\rangle directions, i.e. kϕ>0k_{\phi}>0. [21] For the atomistic spin dynamics, we take three nearest neighbours into account, the first and second nearest neighbour interactions are ferromagnetic and exist between atoms in the same Mn sublattice. The third nearest neighbour interaction is antiferromagnetic between Mn atoms in different sublattices, see App. § 1.4.1 for details.

The Hamiltonian for Py is given by

HPy=−∑i<jSiJijPySj+kcPy2∑i((Six)4+(Siy)4+(Siz)4)+Hd.(3)\mathcal{H}_{\mathrm{Py}}=-\sum_{i<j}\mathbf{S}_{i}J^{\mathrm{Py}}_{ij}\mathbf{S}_{j}+\frac{k_{c}^{\mathrm{Py}}}{2}\sum_{i}\left((S_{i}^{x})^{4}+(S_{i}^{y})^{4}+(S_{i}^{z})^{4}\right)+\mathcal{H}_{d}. \tag*{(3)}

The first term describes the exchange energy of the permalloy, the second term is a weak cubic anisotropy.

The interface Hamiltonian

Hint=−∑i<jSiJijintSj+Hd(4)\mathcal{H}_{\mathrm{int}}=-\sum_{i<j}\mathbf{S}_{i}J^{\mathrm{int}}_{ij}\mathbf{S}_{j}+\mathcal{H}_{d} \tag*{(4)}

acts between the manganese and the permalloy atoms. It leads to a strong coupling between the two layers and imprints the magnetic structures of Mn2_2Au in permalloy. For permalloy [23] as well as for the interface we use a Heisenberg exchange with a nearest neighbour approximation in the atomistic spin dynamics simulations. In App. § 1.4.1 we list the parameters used for the simulations.

For investigations with an external field Bext\mathbf{B}_{\mathrm{ext}}, we add

Hext=−∑iμsSi⋅Bext(5)\mathcal{H}_{\mathrm{ext}}=-\sum_{i}\mu_{s}\mathbf{S}_{i}\cdot\mathbf{B}_{\mathrm{ext}} \tag*{(5)}

to the Hamiltonian H\mathcal{H} in Eq. (1). Note that the external magnetic field is applied to every spin in the system where μs\mu_{s} refers to the spin moment in the respective layer (μPy\mu_{\mathrm{Py}} and μMn\mu_{\mathrm{Mn}} are given in Table I in App. § 1.4.1). As AFMs are largely impervious to magnetic fields, the applied field mostly affects the permalloy. However, due to the strong exchange coupling between the FM and the AFM, the magnetic order in Mn2_2Au is indirectly affected by an applied field as well.

Static properties of single domain states in the bilayer system

We performed Monte Carlo simulations on the pure Mn2_2Au system (for a system size of 8 nm ×\times 8 nm ×\times 5 nm) which reproduced the low-temperature ground state spin structure with the magnetisation of the two Mn sublattices 180 degrees apart, see Figure 1 (c). The easy axes are along the ⟨110⟩\langle110\rangle directions, as expected from the rotational anisotropy and in agreement with previous neutron scattering experiments [24] and theoretical calculations [21, 25].

For the bilayer system (of lateral size 8 nm ×\times 8 nm, and thickness 5 nm of Mn2_2Au and 1nm of permalloy) we find that the ground state of Mn2_2Au is imprinted into the Py as expected due to the strong interlayer exchange coupling [18]. Performing constrained Monte Carlo simulations [26] we computed the energy surfaces for a single domain state in the bilayer system [27]. When a magnetic field is applied the four-fold degeneracy in the energy surface is broken. The applied magnetic field was along the [110] direction, and the energy surface, therefore, favours this easy axis over the other three easy axis directions. To characterise the in-plane spin direction, we introduce the angle ϕ\phi as the angle from the [100] axis in the xyxy plane, see Figure 1. By scanning all angles ϕ\phi we obtain the energy surfaces for varying field strengths as shown in Figure 2. As expected, the field direction, i.e. ϕ=π/4\phi=\pi/4, is energetically preferred. For magnetic field directions perpendicular to the field direction, i.e. ϕ=3π/4\phi=3\pi/4 and ϕ=7π/4\phi=7\pi/4, the energy of the system is independent of the strength of the magnetic field. The easy axis direction which is anti-parallel to the magnetic field, i.e. ϕ=5π/4\phi=5\pi/4, gets enhanced in energy with increasing field strength. A spherical version of Figure 2 can be found in App. B.

Figure 2. Energy surfaces of an Mn₂Au-Py bilayer (average energy per atom) with an applied field of varying strength along the [110] direction, with the critical field Bc≈0.7555 TB_c \approx0.7555\ \mathrm{T}. The MnAu thickness was 5 nm and the permalloy thickness was 1 nm.

The strong in-plane anisotropy of Mn2_2Au and the strong interlayer coupling causes the spins in the two layers to be effectively in-plane. For a single domain state with an applied magnetic field along the [110] direction (as shown in Figure 2), the physics reduces to an effective Hamiltonian Hbilayer\mathcal{H}_{\mathrm{bilayer}} described by the angle ϕ\phi:

Hbilayer(ϕ)=E0+cϕkϕcos⁡4ϕ−cBμPyBextcos⁡(ϕ−π/4).(6)\mathcal{H}_{\mathrm{bilayer}}(\phi)=E_0+c_{\phi}k_{\phi}\cos4\phi-c_B\mu_{\mathrm{Py}}B_{\mathrm{ext}}\cos(\phi-\pi/4). \tag*{(6)}

Here E0E_0 is the energy of the system without the four-fold in-plane anisotropy term. The magnetic field couples to the magnetisation, i.e. the average spin moment of permalloy per atom μPy\mu_{\mathrm{Py}}, in the form of a cos⁡ϕ+sin⁡ϕ\cos\phi+\sin\phi term which can be rewritten as a shifted cosine function, as cos⁡ϕ+sin⁡ϕ=2cos⁡(ϕ−π/4)\cos\phi+\sin\phi=\sqrt{2}\cos(\phi-\pi/4). The constants cϕc_{\phi} and cBc_B depend on the system. cϕc_{\phi} is proportional to the layer thickness of the Mn2_2Au, whereas cBc_B is proportional to the layer thickness of the permalloy.

Upon increasing the magnetic field strength above a critical field value BcB_c, the metastable states (previously oriented approximately perpendicular to the applied field) disappear. At the critical field value BcB_c, the local minima close to ϕ=3π/4\phi=3\pi/4 and 7π/47\pi/4 turn into saddle points, with i) ∂Hbilayer(ϕ)/∂ϕ∣ϕ=ϕ~=0\left.\partial\mathcal{H}_{\mathrm{bilayer}}(\phi)/\partial\phi\right|_{\phi=\tilde{\phi}}=0, ii) ∂2Hbilayer(ϕ)/∂ϕ2∣ϕ=ϕ~=0\left.\partial^2\mathcal{H}_{\mathrm{bilayer}}(\phi)/\partial\phi^2\right|_{\phi=\tilde{\phi}}=0 and iii) ∂3Hbilayer(ϕ)/∂ϕ3∣ϕ=ϕ~=0\left.\partial^3\mathcal{H}_{\mathrm{bilayer}}(\phi)/\partial\phi^3\right|_{\phi=\tilde{\phi}}=0. Solving these two equations close to ϕ=3π/4\phi=3\pi/4 we obtain

Bc=166kϕcϕ9μPycB(7)B_c=\frac{16\sqrt{6}k_{\phi}c_{\phi}}{9\mu_{\mathrm{Py}}c_B} \tag*{(7)}

with ϕ~=3π/4−δϕ≈1.9357\tilde{\phi}=3\pi/4-\delta\phi\approx1.9357 being independent of the model parameters. Using the parameters summarized in App. A) we obtain from the simulation results E0≈−34.1264⋅10−21 J/atomE_0\approx-34.1264\cdot10^{-21}\ \mathrm{J/atom}, cϕ=0.8375c_{\phi}=0.8375 and cB=0.2603c_B=0.2603. For the critical field value, we obtain Bc≈0.7555 TB_c\approx0.7555\ \mathrm{T}.

Domain walls in Mn2Au-Py bilayer systems

In this section, we study a static domain wall across a ribbon bilayer system of dimensions 1000 nm along xx and 40 nm along yy.

along yy. The zz height of MnAu is kept constant at 5 nm, the py height is initially 1 nm, but this is later varied. A 90-degree domain wall from the [110] direction to the [1̄10] direction was initialized at x=100x=100 nm in both the Mn2_2Au and the Py, see Figure 1 and Figure 3a. Our key findings are summarised below: i) The domain wall of Mn2_2Au is imprinted on the permalloy capping. ii) The bilayer structure has a net remaining magnetisation from the permalloy which then allows the observation of domain walls in the AFM via the capping [18]. iii) The permalloy capping increases the average domain wall width of the bilayer system compared to pure Mn2_2Au. iv) The domain wall width varies along the vertical direction, with increasing domain wall width towards the top (i.e. FM surface).

Static domain wall structures in Mn₂Au-Py bilayers

Figure 3. Static domain wall structures in Mn₂Au-Py bilayers. a) Sketch of a 90-degree domain wall. b) Domain wall profiles nxn_x for a 5 nm thick MnAu layer with a 1 nm permalloy capping and without permalloy capping. c) Domain wall widths along the zz direction for varying permalloy capping layer thicknesses.

We computed the domain wall profile of the bilayer using a Monte Carlo integrator. The simulation was run for one million Monte Carlo steps at 0 K until the magnetic structure remained stationary. Figure 3a shows the normalized (height averaged) xx-component of the magnetic order parameter along the ribbon for the bilayer system and a comparison to pure Mn2_2Au. The magnetic order parameter used to model the domain wall profile is the magnetisation for the permalloy and the magnetisation of one sublattice for the Mn2_2Au. We denote this normalized (height averaged) magnetic order parameter by n\mathbf{n}. The domain wall width was extracted by fitting the xx-component, nx=cos⁡Θ(x)n_x = \cos\Theta(x), to the expression of the profile function

Θ(x)=arctan⁡[exp⁡(x−x0δdw)]+π4.(8)\Theta(x) = \arctan\left[\exp\left(\frac{x-x_0}{\delta_{\mathrm{dw}}}\right)\right] + \frac{\pi}{4}. \tag*{(8)}

Here x0x_0 is the position of the domain wall, and δdw\delta_{\mathrm{dw}} the domain wall width. For the 90-degree domain wall, nxn_x varies from nx=1/2n_x = 1/\sqrt{2} on the left, over to nx=0n_x = 0 in the center of the domain wall to nx=−1/2n_x = -1/\sqrt{2} on the right end, as shown in Figure 3a) and Figure 3b).

Our numerical results reveal a domain wall width of δdw≈29.3\delta_{\mathrm{dw}} \approx29.3 nm for the case of pure Mn2_2Au. As the natural domain wall width of permalloy is about an order of magnitude larger, the average domain wall width of the bilayer system depends on the relative thickness of the permalloy to Mn2_2Au. For 1 nm permalloy on top of 5 nm Mn2_2Au, see Figure 3, we obtain a domain wall width of δdw≈38.2\delta_{\mathrm{dw}} \approx38.2 nm, i.e. an increase of about 30%. For such a thin permalloy capping we do not observe a significant change of the domain wall width along the zz direction.

Figure 3c) displays the change of the domain wall width with height (zz-direction) for the device for varying capping layer thicknesses of permalloy. We find that, as expected, i) the domain wall becomes wider towards the FM and ii) there is a larger domain wall width change for thicker permalloy capping. The change in the domain wall width comes from the competition between the magnetocrystaline anisotropy and the exchange interactions, as the exchange interactions and anisotropy vary from bulk MnAu to bulk Py across the interface the domain wall widths vary. For thin Py capping layers the domain wall width in the Py matches the MnAu due to the strong interface exchange coupling.

Manipulating domain walls in Mn2_2Au-Py bilayer systems

In this section, we focus on the dynamics of the previously considered domain walls in Mn2_2Au-Py bilayer systems. Two external driving mechanisms are investigated separately to move the domain wall: an external magnetic field and a current, which induces Néel SOTs.

The system dynamics were calculated by solving the stochastic Landau-Lifshitz-Gilbert equation [28]:

∂Si∂t=−γe1+λ2[Si×Beff+λSi×(Si×Beff)],(9)\frac{\partial\mathbf{S}_i}{\partial t} = -\frac{\gamma_{\mathrm{e}}}{1+\lambda^2}\left[\mathbf{S}_i \times\mathbf{B}_{\mathrm{eff}} + \lambda\mathbf{S}_i \times\left(\mathbf{S}_i \times\mathbf{B}_{\mathrm{eff}}\right)\right], \tag*{(9)}

which models the interaction of an atomic spin moment Si\mathbf{S}_i with an effective field Beff=−δH/δSi\mathbf{B}_{\mathrm{eff}} = -\delta\mathcal{H}/\delta\mathbf{S}_i. The effective field causes the atomic moments to precess around the field, where the frequency of precession is determined by the gyromagnetic ratio of an electron (γe=1.76×1011\gamma_{\mathrm{e}} = 1.76 \times10^{11} rad s−1^{-1}T−1^{-1}). The damping constant λ\lambda is defined in each of the two materials, see Table I in App. § 1.4.1. For our numerical results, Eq. (9) was solved using a Heun scheme [29].

In the following, we considered a 1 nm permalloy capping on top of 5 nm Mn2_2Au. The lateral dimensions of our system remain the same as in Sec. IV, i.e. 1000 nm along xx, 40 nm along yy. Our starting point is a relaxed 90-degree domain wall in the bilayer system from the [110] direction to the [1-10] located at x=100x = 100 nm.

Magnetic field-driven domain wall dynamics

To study the magnetic field-driven domain wall dynamics, we apply a magnetic field along the [110] direction, making this direction the energetically preferred one. To reduce the energy of the bilayer system, the [110] domain in the permalloy is shifted via a domain wall motion. Due to the strong interface exchange coupling between the two layers, the domain wall in the Mn2_2Au is dragged along by the permalloy, leading to a coupled domain wall motion.

We analyse this coupled domain wall motion for different magnetic field strengths. In Figure 4 a) we show snapshots of the domain wall profile at different times for various magnetic field strengths. Besides extending the [110] domain, the field rotates the [1-10] domain such that the xx component of the magnetic order parameter assumes the shifted value of nx=−1/2+δnxn_x = -1/\sqrt{2} + \delta n_x. In Figure 4 b) we display δnx\delta n_x as a function of the applied field strength. At the critical field BcB_c, the domain wall flips to a uniform state, which induces a jump in δnx\delta n_x. This is in agreement with Sec. III, where we find a magnetic field induced shift δϕ\delta\phi in the position of the energy minimum for the domain that is oriented approximately perpendicular to the magnetic field, with δnx=1/2−cos⁡(δϕ−π/2)\delta n_x = 1/\sqrt{2} - \cos(\delta\phi- \pi/2).

Magnetic field-driven domain wall motion for a Py thickness of 1 nm

Figure 4. Magnetic field-driven domain wall motion for a Py thickness of 1 nm; a) domain wall profile snapshots for varying field strengths. This is a height-averaged magnetisation of one AFM sublattice. b) Change in domain orientation δnx\delta n_x as a function of magnetic field strength. c) domain wall velocity as a function of applied field strength.

In Figure 4 c) we show the domain wall velocities as a function of the applied magnetic field strength. As expected, the domain wall moves faster for stronger applied fields. The existence of a critical magnetic field above which the domain wall is flipped into a single domain state, however, puts a boundary on the maximally possible domain wall speed induced by magnetic fields. In our numerics, the magnetic field-driven domain walls have velocities between 0.1 - 8.5 km/s with maximum possible values of 8.5 km/s close to BcB_c.

Néel spin-orbit torque driven domain wall dynamics

In the Mn2_2Au-Py bilayers the SOTs are induced by the Au atoms. The Au atoms cause spin-dependent scattering in the Mn2_2Au and due to the spin symmetry around the Au sites this leads to a Néel SOT acting in opposite directions on the different sublattices. Therefore, the SOTs act only on the Mn atoms and there are no SOTs in the Py capping layer.

To study the domain wall dynamics induced by Néel SOTs, we add the Néel SOT BSOT\mathbf{B}_{\mathrm{SOT}} to the effective field in the LLG equation, Eq. (9)

Beff=−δHδSi+BSOT(10)\mathbf{B}_{\mathrm{eff}} = -\frac{\delta\mathcal{H}}{\delta\mathbf{S}_i} + \mathbf{B}_{\mathrm{SOT}} \tag*{(10)}

where

BSOT=BNTSOT(σ−λS×σ)+BFTSOT(S×σ+λσ),(11)\mathbf{B}_{\mathrm{SOT}}=B_{\mathrm{NT}}^{\mathrm{SOT}}(\boldsymbol{\sigma}-\lambda\mathbf{S}\times\boldsymbol{\sigma})+B_{\mathrm{FT}}^{\mathrm{SOT}}(\mathbf{S}\times\boldsymbol{\sigma}+\lambda\boldsymbol{\sigma}), \tag*{(11)}

comprises both the field-like (BFTSOTB_{\mathrm{FT}}^{\mathrm{SOT}}) and damping like Néel SOTs (BNTSOTB_{\mathrm{NT}}^{\mathrm{SOT}}) [30, 31] acting on the Mn2_2Au layers. The SOTs act in opposite directions in each Mn sublattice due to the spin splitting off the Au atoms. The directions of the SOTs are defined by the spin polarisation unit vector σ\boldsymbol{\sigma}. The spin polarisation unit vector acts perpendicular to the electron flow. Here the electron flow is along [001], and the SOTs acts along [110] and [-1-10] in the two Mn sublattices respectively, effectively shifting the domain wall along the [100] axis. The SOT field strengths BFTSOTB_{\mathrm{FT}}^{\mathrm{SOT}} and BNTSOTB_{\mathrm{NT}}^{\mathrm{SOT}} for an atomistic monolayer are given by [30]

BFTSOT=ℏjeθSHa22eμMn(12)B_{\mathrm{FT}}^{\mathrm{SOT}}=\frac{\hbar j_{\mathrm{e}}\theta_{\mathrm{SH}}a^2}{2e\mu_{\mathrm{Mn}}} \tag*{(12)}
BNTSOT=βSOTBFTSOT(13)B_{\mathrm{NT}}^{\mathrm{SOT}}=\beta_{\mathrm{SOT}}B_{\mathrm{FT}}^{\mathrm{SOT}} \tag*{(13)}

where jej_{\mathrm{e}} is the injected current density and aa is the unit cell size. The spin Hall angle θSH\theta_{\mathrm{SH}} gives the conversion efficiency of electrical current into spin current. βSOT\beta_{\mathrm{SOT}} is an empirical scaling factor that relates the strength of the precessional term with the relaxation term, here assumed to equal one.

In Figure 5a we show the domain wall profiles at 0.00 ns, 0.01 ns, and 0.02 ns for low to higher spin current strengths; je=0.049j_{\mathrm{e}}=0.049 MA/cm2^2, 0.098 MA/cm2^2 and 0.196 MA/cm2^2 corresponding to BNTSOT=0.01B_{\mathrm{NT}}^{\mathrm{SOT}}=0.01 T, 0.02 and 0.04. As expected, for higher spin current strengths the current causes deformations in the shape of the domain wall profile over time. After the initial transient dynamics due to switching on the current, the domain wall reaches a steady state shape and motion in which we compute the domain wall velocity as the average of the gradient of position vs. time. For our chosen parameters we find the maximum velocity of Néel SOT-driven domain walls to be again close to 8.5 km/s even for low currents on the order of 1 MA/cm2^2.

Current driven domain wall motion for a Py thickness of 1 nm

Figure 5. Current driven domain wall motion for a Py thickness of 1 nm; a) domain wall profile snapshots for varying currents. Domain wall profile snapshots for varying current strengths. This is a height-averaged magnetisation of one AFM sublattice. b) domain wall velocity as a function of applied field strength.

Discussion and Summary

We have shown that bilayer systems consisting of a thin permalloy capping on top of Mn2_2Au display strongly coupled domain wall structures, where the domain wall structure of the AFM is imprinted on the FM. A clear advantage of the thin permalloy capping is that the magnetic dynamics of Mn2_2Au become experimentally observable via the magnetisation of the permalloy [18]. Furthermore, we have shown that the coupled magnetic textures can be manipulated by two mechanisms: i) magnetic fields and ii) Néel SOTs. While the applied magnetic field acts mainly in the permalloy, the Néel SOTs act in the Mn2_2Au. In both cases, the strong coupling between the layers causes the spin dynamics in one layer to affect the spin dynamics in the other layer which finally induces a collective domain wall motion. Notably the domain wall motion is independent of the driving mechanism and the material it originated. For both, magnetic field and Néel SOT-driven domain walls we obtain velocities on the order of 8.5 km/s. Such a controlled manipulation of the AFM is a key requirement for AFM-based high-density storage and efficient THz information and computing technologies.

Acknowledgements

We thank Richard Evans, Ricardo Rama-Eiroa, Rubén M. Otxoa, Roy Chantrell, Martin Jourdan, and Satya Prakash Bommanaboyena for fruitful discussions. We acknowledge funding from the German Research Foundation (DFG) - TRR 173 – 268565370 Spin + X: spin in its collective environment (project B12 and A05), Project No. 320163632 (Emmy Noether), CRC/TRR 270 - 405553726 This project made use of the MAGNITUDE cluster, a high-performance computing facility provided by the University of Duisburg-Essen.

Simulation Details

The parameters used for the atomistic simulations are summarised in Table I and explained in more detail below.

InteractionJxxJ_{xx}JyyJ_{yy}JzzJ_{zz}Unit
J1Mn2Au\mathrm{J}_{1}^{\mathrm{Mn_2Au}}-1.094296-1.094296-1.08691110−2010^{-20} J (per link)
J2Mn2Au\mathrm{J}_{2}^{\mathrm{Mn_2Au}}-1.469234-1.469234-1.45931910−2010^{-20} J (per link)
J3Mn2Au\mathrm{J}_{3}^{\mathrm{Mn_2Au}}0.3182610.3182610.31826110−2010^{-20} J (per link)
J~1Mn2Au\tilde{\mathrm{J}}_{1}^{\mathrm{Mn_2Au}}0.00.00.00738510−2010^{-20} J (per link)
J~2Mn2Au\tilde{\mathrm{J}}_{2}^{\mathrm{Mn_2Au}}0.00.00.00991510−2010^{-20} J (per link)
J~3Mn2Au\tilde{\mathrm{J}}_{3}^{\mathrm{Mn_2Au}}0.00.00.31826110−2010^{-20} J (per link)
J~Py\tilde{\mathrm{J}}^{\mathrm{Py}}0.0099150.0099150.00991510−2010^{-20} J (per link)
J~int\tilde{\mathrm{J}}^{\mathrm{int}}0.3182610.3182610.31826110−2010^{-20} J (per link)
ParameterValueUnit
a,ba,b3.327Å
cc8.539Å
μMn\mu_{\mathrm{Mn}}4.0μB\mu_{\mathrm{B}}
μPy\mu_{\mathrm{Py}}1.6μB\mu_{\mathrm{B}}
k4Mn2Auk_{4}^{\mathrm{Mn_2Au}}−1.60218×10−24-1.60218 \times10^{-24}J/atom
kϕMn2Auk_{\phi}^{\mathrm{Mn_2Au}}8.00109×10−258.00109 \times10^{-25}J/atom
kcPyk_{c}^{\mathrm{Py}}1.0×10−261.0 \times10^{-26}J/atom
λMn2Au\lambda_{\mathrm{Mn_2Au}}0.01−-
λPy\lambda_{\mathrm{Py}}0.01−-

Table 1. Model parameters for Mn2_2Au used in the simulations. Isotropic exchange parameters are taken from Khmelevskyi et al. [32] and magnetic anisotropies are taken from Shick et al. [21]. The magnetic moment of the Mn sites is taken from experimental measurements of Barthem et al. [24].

The crystal structure of Mn2_2Au with unit cell dimensions a,ba,b and cc is shown in Figure 6. J1J_1, J2J_2 and J3J_3 indicate the isotropic exchange parameters for the nearest neighbour, next nearest neighbour, and next-next nearest neighbour, at distances 2.180 Å, 2.853 Å, and 3.327 Å, respectively.

Crystal structure of Mn$_2$Au including the nearest, next, and next-next nearest neighbour interactions

Figure 6. Crystal structure of Mn2_2Au including the nearest, next, and next-next nearest neighbour interactions.

In the simulations for the isotropic exchange in Mn2_2Au, the exchange interactions were taken into account up to the next-next nearest neighbour with parameters from Khmelevskyi et al. [32]. The magnetic anisotropies are taken from Shick et al. [21] and the magnetic moment of the manganese sites is taken from experimental measurements of Barthem et al. [24].

For permalloy, we consider only the nearest neighbour FM interaction and the weak cubic anisotropy with kcPyk_{c}^{\mathrm{Py}} taken from Ellis et al. [33].

For the interface between Mn2_2Au and permalloy, we chose an exchange constant of Jint=0.31×10−20J^{\mathrm{int}} = 0.31 \times10^{-20} being roughly 20% of the bulk exchange value of Mn2_2Au. This value is motivated by recent experiments where the interface coupling has been found to be strong [18]. For the damping parameters λPy\lambda_{\mathrm{Py}} and λMn2Au\lambda_{\mathrm{Mn_2Au}} we used 0.01 if not stated otherwise.

Single Domain states / spherical version

Figure 7 shows the spherical version of Figure 2 of the main text. It reveals the transition from the four-fold rotational symmetry in the absence of a magnetic field, to a remaining mirror symmetry in the direction of the magnetic field.

Spherical plot of energy surfaces of an Mn$_2$Au-Py bilayer

Figure 7. Spherical plot of energy surfaces of an Mn2_2Au-Py bilayer (average energy per atom) with an applied field of varying strength along the [110] direction. Larger radii correspond to larger energies.

References

References

  1. [4]V. Baltz, A. Manchon, M. Tsoi, T. Moriyama, T. Ono, and Y. Terskhovnyak, Antiferromagnetic spintronics, Rev. Mod. Phys. 90, 015005 (2018).DOI
  2. [5]T. Jungwirth, J. Sinova, A. Manchon, X. Marti, J. Wunderlich, and C. Felser, The multiple directions of antiferromagnetic spintronics, Nature Physics 14, 200 (2018).DOI
  3. [6]M. B. Jungfleisch, W. Zhang, and A. Hoffmann, Perspectives of antiferromagnetic spintronics, Physics Letters A 382, 865 (2018).DOI
  4. [7]S. Fukami, V. O. Lorenz, and O. Gomonay, Antiferromagnetic spintronics, Journal of Applied Physics 128, 070401 (2020).DOI
  5. [8]P. Wadley, B. Howells, J. Železný, C. Andrews, V. Hills, R. P. Campion, V. Novák, K. Olejník, F. Maccherzzi, S. S. Dhesi, S. Y. Martin, T. Wagner, J. Wunderlich, F. Freimuth, Y. Mokrousov, J. Kuneš, J. S. Chauhan, M. J. Grzybowski, A. W. Rushforth, K. W. Edmonds, B. L. Gallagher, and T. Jungwirth, Electrical switching of an antiferromagnet, Science 351, 587 (2016).DOI
  6. [9]K. Olejník, V. Schuler, X. Marti, V. Novák, Z. Kašpar, P. Wadley, R. P. Campion, K. W. Edmonds, B. L. Gallagher, J. Garces, M. Baumgartner, P. Gambardella, and T. Jungwirth, Antiferromagnetic CuMnAs multi-level memory cell with microelectronic compatibility, Nature Communications 8 (2017).DOI
  7. [10]K. Olejník, T. Seifert, Z. Kašpar, V. Novák, P. Wadley, R. P. Campion, M. Baumgartner, P. Gambardella, P. Němec, J. Wunderlich, J. Sinova, P. Kůžel, M. Müller, T. Kampfrath, and T. Jungwirth, Terahertz electrical switching speed in an antiferromagnetic memory, Science Advances 4 (2018).
  8. [11]T. Matalla-Wagner, M.-F. Rath, D. Graulich, J.-M. Schmalhorst, G. Reiss, and M. Meinert, Electrical Néel-order switching in magnetron-sputtered CuMnAs thin films, Phys. Rev. Applied 12, 064003 (2019).
  9. [12]M. Meinert, D. Graulich, and T. Matalla-Wagner, Electrical switching of antiferromagnetic Mn₂Au and the role of thermal activation, Phys. Rev. Applied 9, 064040 (2018).DOI
  10. [13]Y. Behovits, A. L. Chekhov, S. Y. Bodnar, O. Gueckstock, S. Reimers, Y. Lytvynenko, Y. Skourski, M. Wolf, T. S. Seifert, O. Gomonay, M. Kläui, M. Jourdan, and T. Kampfrath, Terahertz néel spin-orbit torques drive nonlinear magnon dynamics in antiferromagnetic Mn2Au, Nature Communications 14, 6038 (2023).
  11. [14]Y. Cheng, S. Yu, M. Zhu, J. Hwang, and F. Yang, Electrical switching of tristate antiferromagnetic Néel order in α-Fe₂O₃ epitaxial films, Phys. Rev. Lett. 124, 027202 (2020).
  12. [15]T. Hajiri, S. Ishino, K. Matsuura, and H. Asano, Electrical current switching of the noncollinear antiferromagnet Mn₃GaN, Applied Physics Letters 115, 052403 (2019).
  13. [16]M. Dunz, T. Matalla-Wagner, and M. Meinert, Spin-orbit torque induced electrical switching of antiferromagnetic MnN, Phys. Rev. Research 2, 013347 (2020).DOI
  14. [17]J. Shi, V. Lopez-Dominguez, F. Garesci, C. Wang, H. Almasi, M. Grayson, G. Finocchio, and P. K. Amiri, Electrical manipulation of the magnetic order in antiferromagnetic PtMn pillars, Nature Electronics 3, 92 (2020).
  15. [18]S. P. Bommanaboyena, D. Backes, L. S. I. Veiga, S. S. Dhesi, Y. R. Niu, B. Sarpi, T. Denneulin, A. Kovács, T. Mashoff, O. Gomonay, J. Sinova, K. Kläui, M. Jourdain, K. Everschor-Sitte, D. Schönke, R. M. Reeve, M. Kläui, H.-J. Elmers, and M. Jourdan, Readout of an antiferromagnetic spintronics system by strong exchange coupling of Mn₂Au and permalloy, Nature Communications 12, 6539 (2021).
  16. [19]H. Al-Hamdo, T. Wagner, Y. Lytvynenko, G. Kendzo, S. Reimers, M. Ruhwedel, M. Yaqoob, V. I. Vasyuchka, P. Pirro, J. Sinova, M. Kläui, M. Jourdan, O. Gomonay, and M. Weiler, Coupling of ferromagnetic and antiferromagnetic spin dynamics in mn₂Au/NiFe thin film bilayers, Phys. Rev. Lett. 131, 046701 (2023).DOI
  17. [20]P. Wadley, K. W. Edmonds, M. R. Shahedkhah, R. P. Campion, B. L. Gallagher, J. Železný, J. Kuneš, V. Novák, T. Jungwirth, V. Saidl, P. Němec, F. Maccherzzi, and S. S. Dhesi, Control of antiferromagnetic spin axis orientation in bilayer fe/cumnas films, Scientific Reports 7, 11147 (2017).arxiv.org/abs/1702.03147
  18. [21]A. B. Shick, S. Khmelevskyi, O. N. Mryasov, J. Wunderlich, and T. Jungwirth, Spin-orbit coupling induced anisotropy effects in bimetallic antiferromagnets: A route towards antiferromagnetic spintronics, Phys. Rev. B 81, 212409 (2010).
  19. [22]R. F. L. Evans, L. Rózsa, S. Jenkins, and U. Atxitia, Temperature scaling of two-ion anisotropy in pure and mixed anisotropy systems, Phys. Rev. B 102, 020412 (2020).
  20. [23]D. Meilak, S. Jenkins, R. Pond, and R. F. L. Evans, Massively parallel atomistic simulation of ultrafast thermal spin dynamics of a permalloy vortex (2019), arXiv:1908.08885.
  21. [24]V. Barthem, C. Colin, H. Mayaffre, M.-H. Julien, and D. Givord, Revealing the properties of Mn₂Au for antiferromagnetic spintronics, Nature Communications 4 (2013).DOI
  22. [25]J. Hirst, U. Atxitia, S. Ruta, J. Jackson, L. Petit, and T. Ostler, Temperature-dependent micromagnetic model of the antiferromagnet mn₂Au: A multiscale approach, Phys. Rev. B 106, 094402 (2022).DOI
  23. [26]P. Asselin, R. F. L. Evans, J. Barker, R. W. Chantrell, R. Yanes, O. Chubykalo-Fesenko, D. Hinzke, and U. Nowak, Constrained Monte Carlo method and calculation of the temperature dependence of magnetic anisotropy, Physical Review B 82, 054415 (2010).
  24. [27]We constrained the direction of the magnetisation of a single Mn sublattice while allowing all other spins to relax to their equilibrium spin structures.
  25. [28]J. L. Garcia-Palacios and F. J. Lázaro, Langevin-dynamics study of the dynamical properties of small magnetic particles, Physical Review B 58, 14937 (1998).
  26. [29]R. F. L. Evans, W. J. Fan, P. Chureemart, T. A. Ostler, M. O. A. Ellis, and R. W. Chantrell, Atomistic spin model simulations of magnetic nanomaterials, J. Phys.: Condens. Matt. 26, 103202 (2014).
  27. [30]A. Manchon, J. Železný, I. M. Miron, T. Jungwirth, J. Sinova, A. Thiaville, K. Garello, and P. Gambardella, Current-induced spin-orbit torques in ferromagnetic and antiferromagnetic systems, Reviews of Modern Physics 91, 035004 (2019).
  28. [31]A. Meo, C. E. Cronshaw, S. Jenkins, A. Lees, and R. F. L. Evans, Spin-transfer and spin-orbit torques in the Landau–Lifshitz–Gilbert equation, Journal of Physics: Condensed Matter 35, 025801 (2022).
  29. [32]S. Khmelevskyi and P. Mohn, Layered antiferromagnetism with high Néel temperature in the intermetallic compound Mn₂Au, Applied Physics Letters 93, 162503 (2008).
  30. [33]M. O. A. Ellis, T. A. Ostler, and R. W. Chantrell, Classical spin model of the relaxation dynamics of rare-earth doped permalloy, Phys. Rev. B 86, 174418 (2012).DOI

Paper details

vlnc:W_7wnsytbn
Version
v1 · latest
Published
Fresh — added to the Hub within the last 30 days
Added
License
CC BY 4.0
Usage

views · 0

downloads · 0

A view counts once per browser per day, a download each time the PDF is requested.

  • Physics and Astronomy

Not recorded for this paper

View statement
Looking for related papers…
Contents