betaFeedback

WorksPhysics and Astronomy

Mixed-Salt Enhanced Chemical Vapor Deposition of Two-Dimensional Transition Metal Dichalcogenides

Abstract

The usage of molten salts, e.g., Na2MoO4 and Na2WO4, has shown great success in the growth of two-dimensional (2D) transition metal dichalcogenides (TMDCs) by chemical vapor deposition (CVD). In comparison with the halide salt (i.e., NaCl, NaBr, KI)-assisted growth (Salt 1.0), the molten salt-assisted vapor-liquid-solid (VLS) growth technique (Salt 2.0) has improved the reproducibility, efficiency and scalability of synthesizing 2D TMDCs. However, the growth of large-area MoSe2 and WTe2 is still quite challenging with the use Salt 2.0 technique. In this study, a renewed Salt 2.0 technique using mixed salts (e.g., Na2MoO4-Na2SeO3 and Na2WO4-Na2TeO3) is developed for the enhanced CVD growth of 2D MoSe2 and WTe2 crystals with large grain size and yield. Continuous monolayer MoSe2 film with grain size of 100-250 μm or isolated flakes up to ~ 450 μm is grown on a halved 2-inch SiO2/Si wafer. Our study further confirms the synergistic effect of Na+ and SeO32- in the enhanced CVD growth of wafer-scale monolayer MoSe2 film. And thus, the addition of Na2SeO3 and Na2TeO3 into the transition metal salts could be a general strategy for the enhanced CVD growth of many other 2D selenides and tellurides.

Mixed Salt CVD_MS_210824

Image not extracted

Figure 1. Boosting growth of MoSe2_2 with Na2_2SeO3_3. An enhanced CVD growth of continuous MoSe2_2 film was achieved by adding Na2_2SeO3_3 to Na2_2MoO4_4. This work provides a general strategy for large-area growth of 2D transition metal dichalcogenides using mixed molten salts.

Abstract

The usage of molten salts, e.g., Na2_2MoO4_4 and Na2_2WO4_4, has shown great success in the growth of two-dimensional (2D) transition metal dichalcogenides (TMDCs) by chemical vapor deposition (CVD). In comparison with the halide salt (i.e., NaCl, NaBr, KI)-assisted growth (Salt 1.0), the molten salt-assisted vapor-liquid-solid (VLS) growth technique (Salt 2.0) has improved the reproducibility, efficiency and scalability of synthesizing 2D TMDCs. However, the growth of large-area MoSe2_2 and WTe2_2 is still quite challenging with the use Salt 2.0 technique. In this study, a renewed Salt 2.0 technique using mixed salts (e.g., Na2_2MoO4_4-Na2_2SeO3_3 and Na2_2WO4_4-Na2_2TeO3_3) is developed for the enhanced CVD growth of 2D MoSe2_2 and WTe2_2 crystals with large grain size and yield. Continuous monolayer MoSe2_2 film with grain size of 100-250 μm or isolated flakes up to ∼ 450 μm is grown on a halved 2-inch SiO2_2/Si wafer. Our study further confirms the synergistic effect of Na+^{+} and SeO32−_3^{2-} in the enhanced CVD growth of wafer-scale monolayer MoSe2_2 film. And thus, the addition of Na2_2SeO3_3 and Na2_2TeO3_3 into the transition metal salts could be a general strategy for the enhanced CVD growth of many other 2D selenides and tellurides.

Introduction

Two-dimensional (2D) layered transition-metal dichalcogenides (TMDCs) with unique electrical properties are promising materials for future electronic devices. Among them, the semiconducting TMDCs (e.g., MoS2_2, MoSe2_2, WSe2_2, etc.) are idea channel materials for field effect transistors (FETs) because of their high carrier mobility and current on/off ratio, which may reach from tens to hundreds cm2^2/Vs and up to 108^8, respectively.[1, 2, 3] Meanwhile, the metallic TMDCs (e.g., VSe2\mathrm{VSe}_2, VTe2\mathrm{VTe}_2, WTe2\mathrm{WTe}_2, etc.)[4, 5, 6, 7] also play important roles in future all-2D integrated circuits as contacts and interconnects.[8] To realize their potential application in 2D electronics, the TMDCs should be prepared with high crystallinity, uniformity and reproducibility at low cost.

In the past decade, many growth techniques were employed for the synthesis of 2D TMDCs, from chemical vapor transport (CVT) growth of bulk TMDC crystals to the pioneering chemical vapor deposition (CVD) growth of MoS2\mathrm{MoS}_2, and then metal organic (MO) CVD synthesis of large-area 2D TMDCs.[9, 10, 11, 12] Among these approaches, CVD is the most promising method due to its low cost, easy controllability, and scalability for mass production.

The typical CVD growth of 2D TMDCs usually involves the powders of transition metal oxides and chalcogen precursors, where the 2D TMDCs are grown via a vapor-solid-solid (VSS) growth mechanism. However, some oxides (e.g., WO3\mathrm{WO}_3 and Nb2O5\mathrm{Nb}_2\mathrm{O}_5) with high melting points close to 1500 ∘C1500\,^\circ\mathrm{C} are hard to vaporize at the common growth temperature of 700700-900 ∘C900\,^\circ\mathrm{C}.[13] To solve this issue, we first introduced halides (e.g., NaCl, NaBr, KI, etc.) as growth promoters to facilitate the growth of large WS2\mathrm{WS}_2 and WSe2\mathrm{WSe}_2 monolayers.[14] Such improved CVD growth is attributed to the in-situ generated oxyhalides, which have low melting points around 300 ∘C300\,^\circ\mathrm{C} and thus providing sufficient high vapor pressure for the feasible growth of 2D TMDCs. This Salt 1.0 technique had succeeded in growing tens different kinds of layered metal chalcogenides and their alloys/junctions.[15] A recent study found that the fluoride can also facilitate the growth of graphene and h-BN monolayers.[16] However, the Salt 1.0 technique following the VSS growth mechanism has several intrinsic drawbacks, which include non-uniform metal precursor (vapor) distribution on the growth substrate, poor coverage uniformity and reproducibility, and contamination on growth chambers. These cause the wafer-scale and patterned growth of TMDCs almost impossible. Furthermore, extra costs are needed to replace the contaminated growth chambers/tubes frequently.

Until recently, Salt 2.0 technique has been developed to enable the CVD growth of 1D and 2D TMDCs via a vapor-liquid-solid (VLS) mechanism.[17, 18, 19, 20] This method uses the molten salts, e.g., Na2_2Mo2_2O7_7, Na2_2MoO4_4, Na2_2WO4_4, NaReO4_4, NaVO3_3, etc., which have melting points close to the typical TMDC growth temperatures (650-850 °C). During the reaction, these transition metal salts are in molten liquid state, which is essentially different from those in the Salt 1.0 technique. The molten salts have the advantage to be prepared in stable aqueous solutions that can either be uniformly deposited on large wafers via spin-coating or to form patterns on substrates. We had indeed demonstrated 2-inch wafer-scale and deterministic patterned growth of MoS2_2 and WS2_2 monolayers using Na2_2MoO4_4 and Na2_2WO4_4 aqueous solutions, respectively.[18, 19] Zuo et al., also demonstrated the growth of MoS2_2, MoSe2_2, WS2_2 and WSe2_2 inside the channels of optical fibers using the Salt 2.0 technique, resulting in an ultrahigh nonlinearity ever achieved.[21] In addition, we also demonstrated the CVD growth of rhenium (Re) and vanadium (V)-doped TMDCs by simply mixing molten salt aqueous solutions in designated ratios. These CVD-grown Re- and V-doped TMDCs with tunable dopants concentrations, electrical and optical properties are highly promising for future electronic and optoelectronics.[22] The Salt 2.0 technique is hence, highly promising towards the practical application of 2D TMDC-based electronics.

In this paper, we report an enhanced CVD growth of 2D MoSe2_2, ReSe2_2 and WTe2_2, which are still quite challenging to grow with the Salt 2.0 technique using Na2_2MoO4_4, NaReO4_4, and Na2WO4\mathrm{Na}_2\mathrm{WO}_4 only. By using mixed transition metal salts and halogen salts, e.g., Na2MoO4\mathrm{Na}_2\mathrm{MoO}_4-Na2SeO3\mathrm{Na}_2\mathrm{SeO}_3, NaReO4\mathrm{NaReO}_4-Na2SeO3\mathrm{Na}_2\mathrm{SeO}_3 and Na2WO4\mathrm{Na}_2\mathrm{WO}_4-Na2TeO3\mathrm{Na}_2\mathrm{TeO}_3, much improved growth of MoSe2\mathrm{MoSe}_2, ReSe2\mathrm{ReSe}_2 and WTe2\mathrm{WTe}_2 is achieved, respectively. The most substantial achievement lies in the growth of continuous MoSe2\mathrm{MoSe}_2 film on a halved 2-inch SiO2/Si\mathrm{SiO}_2/\mathrm{Si} wafer with large grain sizes of 100-250 μm\mu\mathrm{m} or isolated flakes up to ∼450\sim450 μm\mu\mathrm{m} using the Na2MoO4\mathrm{Na}_2\mathrm{MoO}_4-Na2SeO3\mathrm{Na}_2\mathrm{SeO}_3, which is much better than that grown using Na2MoO4\mathrm{Na}_2\mathrm{MoO}_4 only. Similarly, the ReSe2\mathrm{ReSe}_2 and WTe2\mathrm{WTe}_2 also show much improved yield and grain size with the addition of Na2SeO3\mathrm{Na}_2\mathrm{SeO}_3 and Na2TeO3\mathrm{Na}_2\mathrm{TeO}_3, respectively. Our theoretical studies indicate that the growth of 2D Se- and Te-based TMDCs is thermodynamically favored when the chalcogen salts are introduced. The chalcogen salts added can effectively decrease the formation energies of 2D TMDCs. Such enhanced CVD growth using mixed salts strategy therefore provides a robust synthetic alternative for many 2D selenides and tellurides towards future electronics.

RESULTS AND DISSCUSSIONS

Strategy for enhanced CVD growth of 2D TMDCs using mixed salt precursors

The successful growth of 2D TMDCs with the Salt 2.0 technique requires a careful choice of salt precursors. Basically, the molten salts need to meet two main criteria: 1) possess reasonably high melting points; 2) formation of stable aqueous solutions, considering the growth mechanism involved. Take the VLS growth of 1D MoS2\mathrm{MoS}_2 nanoribbons for instance, molten Na-Mo-O salt (Na2Mo2O7\mathrm{Na}_2\mathrm{Mo}_2\mathrm{O}_7) first forms liquid droplets on the growth substrates. Then, the sulfur vapor adsorbs on their surface and diffuses into the droplets, forming Na-Mo-S-O. When the Na-Mo-O-S droplets become supersaturated with sulfur, solid MoS2\mathrm{MoS}_2 nanoribbons are precipitated out finally.[17] And thus, precursors with a suitable range of heat tolerance/stability and easy incorporation of chalcogen are crucial to initiate seeding and to mediate growth.

Figure 1a shows some transition metal salts that have been used for the successful growth of 2D transition metal sulfide.[17, 21, 23] However, it is still quite challenging to grow large-area, high-quality 2D transition metal selenide (e.g., MoSe2\mathrm{MoSe}_{2}) and tellurides (e.g., WTe2\mathrm{WTe}_{2}) using these precursors. We attribute this to the difficult incorporation of chalcogen atoms, especially Se and Te in the transition metal salts to initiate the TMDC nucleation and the subsequent growth.

In previous study, tellurium was mixed with MoO3\mathrm{MoO}_{3}, tungsten and rhenium to promote the growth 2D transition metal sulfides, MoS2\mathrm{MoS}_{2}, WS2\mathrm{WS}_{2} and ReS2\mathrm{ReS}_{2}, respectively.[24, 25] To overcome this, chalcogen salts, e.g., Na2SeO3\mathrm{Na}_{2}\mathrm{SeO}_{3} and Na2TeO3\mathrm{Na}_{2}\mathrm{TeO}_{3} with similar chemical properties (reasonably high melting points and soluble in H2O\mathrm{H}_{2}\mathrm{O}) were added to the transition metal salts to prepare the mixed-salt aqueous solutions. Compared to the molten salts with Na-Mo-O or Na-W-O only, the mixed molten salts containing Na-Mo-Se-O or Na-W-Te-O may assist the nucleation during the temperature ramping process and facilitate the rapid growth of 2D TMDCs when elemental chalcogen vapor is introduced at the growth stage. To confirm this idea, we first prepared the mixed-salt aqueous solutions. Then, the solutions were spin-coated onto the growth substrates. CVD growth was performed in a 2-inch tube furnace with Se or Te powder loaded in the upstream and growth substrates positioned at the center. The synthetic strategy and method are illustrated in Figure 1b and Figure S1.

Image not extracted

Figure S1. Schematic illustrations of the enhanced CVD growth of monolayer MoSe2\mathrm{MoSe}_2 films using mixed Na2MoO4/Na2SeO3\mathrm{Na}_2\mathrm{MoO}_4/\mathrm{Na}_2\mathrm{SeO}_3. (a) The preparation of liquid precursors by dissolving Na2MoO4\mathrm{Na}_2\mathrm{MoO}_4 and Na2SeO3\mathrm{Na}_2\mathrm{SeO}_3 in DI H2O\mathrm{H}_2\mathrm{O}. (b) Depositing mixed salts on growth substrate via spin-coating of the liquid precursor. (c) CVD growth of MoSe2\mathrm{MoSe}_2 films via selenization of the mixed Na2MoO4/Na2SeO3\mathrm{Na}_2\mathrm{MoO}_4/\mathrm{Na}_2\mathrm{SeO}_3 on substrate.

Image not extracted

Figure 1 (PDF p. 8). Enhanced CVD growth of 2D TMDCs with mixed transition metal salts and chalcogen salts. (a) A color bar indicating the melting points of several salt precursors. (b) The synthetic strategy for enhanced CVD growth of wafer-scale 2D MoSe2_2 films with mixed-salt precursors.

Enhanced CVD growth of MoSe2_2 monolayers using mixed Na2_2MoO4_4-Na2_2SeO3_3

To evaluate the proposed strategy for enhanced CVD, we first conducted the growth of MoSe2_2 monolayers using the mixed Na2_2MoO4_4-Na2_2SeO3_3 (16 mM, 1:1) solution. Figure 2a is a photo showing a uniform MoSe2_2 film grown on a halved 2-inch SiO2_2/Si wafer, which has an obvious color contrast different from the bare SiO2_2/Si wafer. Low-magnification optical image shows that the MoSe2_2 film grown with Na2_2MoO4_4-Na2_2SeO3_3 has a full coverage with a fairly low-density of thick-layers (Figure 2b). Our statistical result indicates a high coverage yield of MoSe2_2 monolayer up to ~ 98.3%. A fine control of the mixed salts’ concentrations is anticipated to result in a full coverage of MoSe2_2 monolayer in future. High-magnification optical images reveal that the as-grown MoSe2_2 monolayer has large domain size in the range of 100-250 μ\mum (Figure 2c, Figure S2 and Figure S2). When the Na2_2MoO4_4:Na2_2SeO3_3 molar ratio changes to 1:2, large MoSe2\mathrm{MoSe}_{2} monolayers with a domain size up to ∼450 μm\sim450\ \mu\mathrm{m} are observed (Figure S2). Meanwhile in the controlled growth without adding any Na2SeO3\mathrm{Na}_{2}\mathrm{SeO}_{3}, only small (∼10 μm\sim10\ \mu\mathrm{m}) MoSe2\mathrm{MoSe}_{2} flakes are grown (Figure 2d and Figure S2).

Image not extracted

Figure 2. Characterization of MoSe2_2 monolayers grown with Na2_2MoO4_4-Na2_2SeO3_3. (a) A photo of monolayer MoSe2_2 film grown on a halved 2-inch wafer. (b, c) Optical images of monolayer MoSe2_2 film grown with the mixed salts. The dotted lines indicate the grain boundaries (GB). (d) An optical image of MoSe2_2 grown with Na2_2MoO4_4 only. Inset shows a typical MoSe2_2 flake in an area of 10 ×\times 10 μm2^2. (e) Typical Raman spectrum of the as-grown MoSe2_2 monolayer. (f) OM image and corresponding Raman peak position and intensity maps. (g) Typical PL spectrum of the as-grown MoSe2_2 monolayer. (h) OM image and corresponding PL peak position and intensity maps. (i) A typical ADF-STEM image of the as-grown MoSe2_2 monolayer. The green circles indicate the single and double Se vacancies in the MoSe2_2 lattice. (j) Transport curves of MoSe2_2-FETs. Inset shows the channel area of a MoSe2_2-FET. The data presented in figures e-j were obtained from monolayer MoSe2_2 films grown with the mixed salts.

Image not extracted

Figure S2. Optical images of MoSe2_2 grown on SiO2_2/Si substrates with different Na2_2MoO4_4:Na2_2SeO3_3 ratios. (a) 1:0.5, (b) 1:1, (c) 1:2 and (d) 1:0. Large MoSe2_2 monolayers with grain size in the range of 150 - 450 μ\mum can be grown when using mixed Na2_2MoO4_4-Na2_2SeO3_3 as growth precursors.

Figure 2e is a typical Raman spectrum of as-grown monolayer MoSe2\mathrm{MoSe}_{2} film with the characteristic A1g\mathrm{A}_{1g} peak located at 239.8 cm−1239.8\ \mathrm{cm}^{-1}, which is slightly higher than the strain-free exfoliated MoSe2\mathrm{MoSe}_{2} monolayers, ∼239.5 cm−1\sim239.5\ \mathrm{cm}^{-1}[26]. Figure 2f shows an optical image and corresponding Raman maps of two adjacent monolayer MoSe2\mathrm{MoSe}_{2} domains. The Raman peak position map over a large area of 165×355 μm2165 \times355\ \mu\mathrm{m}^{2} demonstrates a small variation from 238.9238.9 to 239.8 cm−1239.8\ \mathrm{cm}^{-1}. We attribute the Raman peak variation to the strain existed in the CVD-grown monolayer MoSe2\mathrm{MoSe}_{2} film.[27, 28] Nonetheless, the Raman peak intensity map shows a good uniformity. The intensity gradient from the bottom left to top right is attributable to the different focusing conditions encountered in such a large mapping area caused by the uneven substrate/sample stage. Figure 2g is a typical photoluminescence (PL) spectrum of as-grown monolayer MoSe2\mathrm{MoSe}_{2} with a peak position located at ∼837 nm\sim837\ \mathrm{nm} (∼1.481 eV\sim1.481\ \mathrm{eV}) corresponding to the A exciton emission. The small FWHM of ∼40 meV\sim40\ \mathrm{meV} indicates a good optical quality of as-grown monolayer MoSe2\mathrm{MoSe}_{2} film.[26, 29, 30, 31] Figure 2h shows an optical image and corresponding PL maps of two adjacent monolayer MoSe2\mathrm{MoSe}_{2} domains. In the large mapping area of 120×300 μm2120 \times300\ \mu\mathrm{m}^{2}, the PL maps demonstrate small deviation in peak position (photon energy) and peak intensity, indicating a great optical uniformity in such large monolayer MoSe2\mathrm{MoSe}_{2} domains.[29, 30]

The structural analysis performed on the transferred MoSe2\mathrm{MoSe}_{2} monolayer via annular dark-field (ADF) scanning transmission electron microscopy (STEM) reveals that the MoSe2\mathrm{MoSe}_{2} monolayer has a good crystallinity (Figure 2i). A small portion of Se vacancies is observed, possibly due to the hydrogen etching occurred during the cooling process. We further investigated the electrical quality of the as-grown MoSe2\mathrm{MoSe}_{2} monolayers by fabricating FETs (Figure S3-Figure S3). The MoSe2\mathrm{MoSe}_{2}-FETs show typical n-type transport behavior with a high current on/off ratio up to 10810^{8} (Figure 2j). From a total 16 devices measured, they show current on/off ratios around 10810^{8}-10910^{9} and electron mobilities range from 5.2 to 16.4 cm2\mathrm{cm}^{2}/Vs with an average of 8.2 cm2\mathrm{cm}^{2}/Vs (Figure S3). It is noteworthy to mention that the electrical performance of our CVD-grown monolayer MoSe2\mathrm{MoSe}_{2} film is similar or to a certain extent better than the previously reported, CVD-grown isolated flakes and continuous film.[32, 33, 34, 35, 36, 37] Although high-mobility monolayer MoSe2\mathrm{MoSe}_{2} have also been grown by Wang et al. and Li et al.,[29, 38] they are limited only to isolated submillimeter-size flakes. It is therefore crucial to seek a feasible growth that accommodates large-area growth of high-quality MoSe2\mathrm{MoSe}_{2} film. Furthermore, the value obtained is still incomparable to that of the CVD-grown MoS2\mathrm{MoS}_{2} monolayers,[18, 39] the electrical performance, environmental stability and crystallinity of our CVD-grown monolayer MoSe2\mathrm{MoSe}_{2} films can be further improved by using a fast-cooling process with high-flux of Se vapor.[40] Notably, enhanced CVD growth of 2D ReSe2\mathrm{ReSe}_{2} flakes is also achieved via the use of mixed NaReO4\mathrm{NaReO}_{4}-Na2SeO3\mathrm{Na}_{2}\mathrm{SeO}_{3} (Figure S4). It could be a versatile strategy for growing many other 2D metal selenides.

Image not extracted

Figure S3. Monolayer MoSe2_2-FETs. (a) An array of monolayer MoSe2_2-FETs fabricated with MoSe2_2 film transferred on 285 nm SiO2_2 (285 nm)/Si substrate (∼\sim10×\times10 mm2^2). (b, c) Optical images of a single MoSe2_2-FET. Photolithography and oxygen plasma were employed to define the channel shape and etch surrounding MoSe2_2. (d) Statistical result of the electron mobility vs. current on/off ratio for a total of 16 MoSe2_2-FETs measured.

Image not extracted

Figure S4. Characterization of ReSe2\mathrm{ReSe}_{2} grown with mixed NaReO4\mathrm{NaReO}_{4}–Na2SeO3\mathrm{Na}_{2}\mathrm{SeO}_{3}. (a) An optical image showing the as-grown ReSe2\mathrm{ReSe}_{2} flakes on sapphire substrate. (b) An AFM image of the ReSe2\mathrm{ReSe}_{2} flakes transferred onto a SiO2\mathrm{SiO}_{2}/Si substrate. (c) Typical Raman spectrum of the as-grown ReSe2\mathrm{ReSe}_{2} flakes. (d, e) Typical (d) optical image and (e) transport curve of a ReSe2\mathrm{ReSe}_{2}-FET. (f, g) Optical images of as-grown small ReSe2\mathrm{ReSe}_{2} flakes using NaReO4\mathrm{NaReO}_{4} only.

Enhanced CVD growth of WTe2\mathrm{WTe}_{2} using mixed Na2WO4\mathrm{Na}_{2}\mathrm{WO}_{4}-Na2TeO3\mathrm{Na}_{2}\mathrm{TeO}_{3}

We further evaluated the CVD growth of WTe2\mathrm{WTe}_{2} using mixed Na2WO4\mathrm{Na}_{2}\mathrm{WO}_{4}-Na2TeO3\mathrm{Na}_{2}\mathrm{TeO}_{3} and Na2WO4\mathrm{Na}_{2}\mathrm{WO}_{4} only. Figure 3a and 3b are optical images of few-layer WTe2\mathrm{WTe}_{2} flakes grown on sapphire substrate with Na2WO4\mathrm{Na}_{2}\mathrm{WO}_{4}-Na2TeO3\mathrm{Na}_{2}\mathrm{TeO}_{3} (30 mM, 1:1). In contrast to the thick, small flakes grown (Figure 3c and inset), addition of the Na2TeO3\mathrm{Na}_{2}\mathrm{TeO}_{3} results in the growth of thin WTe2\mathrm{WTe}_{2} of much larger size (Figure 3a and 3b). Figure 3d is an atomic force microscope (AFM) image obtained from a WTe2\mathrm{WTe}_{2} flake grown with the mixed salts. Most of the WTe2\mathrm{WTe}_{2} flakes have a height of ∼2.1\sim2.1 nm, corresponding to a tri-layer structure (Figure 3d). A typical Raman spectrum of as-grown WTe2\mathrm{WTe}_{2} flake on sapphire substrate is presented in Figure 3e. Five characteristic peaks located at 110.7 cm−1^{-1}, 116.6 cm−1^{-1}, 134.0 cm−1^{-1}, 163.0 cm−1^{-1}, and 211 cm−1^{-1} are well-matched to the Raman active modes (A24A^{4}_{2}, A13A^{3}_{1}, A15A^{5}_{1}, A17A^{7}_{1}, A19A^{9}_{1}) of T′T^{\prime}-WTe2\mathrm{WTe}_{2}.[41] Figure 3f shows a typical high-resolution ADF-STEM image and the atomic structure of T′T^{\prime}-WTe2\mathrm{WTe}_{2}. The typical transport curve of a tri-layer WTe2\mathrm{WTe}_{2}-FET in Figure 3g shows good metallic transport behaviour with poor gate dependency and high conductivity. It could be a promising contact material for future 2D electronics.[6, 7]

Image not extracted

Figure 3. Characterization of the WTe2_2 grown with Na2_2WO4_4-Na2_2TeO3_3. (a, b) Optical images of few-layer WTe2_2 grown with the mixed Na2_2WO4_4-Na2_2TeO3_3. (c) An optical image of the WTe2_2 grown with Na2_2WO4_4 only. Inset shows a single WTe2_2 flake in an area of 10 × 10 μm2^2. (d) AFM image and height profile of a WTe2_2 flake. (e) Raman spectra of as-grown T′-WTe2_2. (f) Typical ADF-STEM image and atomic models of as-grown T′-WTe2_2. (g) Typical transport curve of a tri-layer WTe2_2-FET. Inset shows the optical image of the channel area. Data in figure d-g were obtained from the WTe2_2 flakes grown with the mixed salts.

The mechanism for improved CVD growth of 2D TMDCs with mixed salts

To reveal the mechanism for such enhanced CVD growth using mixed salts, we compared the MoSe2_2 growth in separate sets of experiments to identify the functions of SeO32−_3^{2-} and Na+^+, respectively.

First, we clarify the effectiveness of SeO32−_3^{2-} by using salt precursors without/with SeO32−_3^{2-} at fixed Na+^+ and MoO42−_4^{2-} molar ratio, i.e. Na2_2MoO4_4 (16 mM) and (NH4_4)2_2MoO4_4-Na2_2SeO3_3 (16 mM, 1:1). Figure 4a shows a halved 2-inch SiO2\mathrm{SiO}_{2}/Si wafer fully covered with a uniform MoSe2\mathrm{MoSe}_{2} film grown with (NH4)2MoO4(\mathrm{NH}_{4})_{2}\mathrm{MoO}_{4}-Na2SeO3\mathrm{Na}_{2}\mathrm{SeO}_{3}, where Na+:MoO42−:SeO32−=2:1:1\mathrm{Na}^{+}:\mathrm{MoO}_{4}^{2-}:\mathrm{SeO}_{3}^{2-}=2:1:1. Optical images show that the as-grown MoSe2\mathrm{MoSe}_{2} film comprises mainly of continuous monolayers with small portion of voids and thick layers (Figure 4b and 4c). The as-grown MoSe2\mathrm{MoSe}_{2} film also shows uniform Raman (Figure 4d) and PL spectra (Figure 4e) over the whole wafer. Furthermore, this mixed salts also demonstrate high growth reproducibility (Figure S5-Figure S5). Compared to the growth using Na2MoO4\mathrm{Na}_{2}\mathrm{MoO}_{4} only with the same Na+:MoO42−\mathrm{Na}^{+}:\mathrm{MoO}_{4}^{2-} molar ratio of 2:1 (Figure 2d), the addition of SeO32−\mathrm{SeO}_{3}^{2-} can effectively improve the growth of MoSe2\mathrm{MoSe}_{2} monolayers. This further confirms the effectiveness of chalcogen salts in the enhanced CVD growth of 2D TMDCs. It is important to mention that the enhanced MoSe2\mathrm{MoSe}_{2} growth using (NH4)2MoO4(\mathrm{NH}_{4})_{2}\mathrm{MoO}_{4}-Na2SeO3\mathrm{Na}_{2}\mathrm{SeO}_{3} is not caused by the change of transition metal salts, from Na2MoO4\mathrm{Na}_{2}\mathrm{MoO}_{4} to (NH4)2MoO4(\mathrm{NH}_{4})_{2}\mathrm{MoO}_{4}. In controlled experiments, there is no MoSe2\mathrm{MoSe}_{2} observed when only (NH4)2MoO4(\mathrm{NH}_{4})_{2}\mathrm{MoO}_{4} is used (Figure S5 and S5b).

Image not extracted

Figure 4. Contribution of SeO32−_3^{2-} and Na+^{+} in the MoSe2_2 growth with mixed salts. (a) A photo of monolayer MoSe2_2 film grown on a halved 2-inch SiO2_2/Si wafer with (NH4_4)2_2MoO4_4-Na2_2SeO3_3 (16mM, 1:1). (b, c) Optical images of monolayer MoSe2_2 film grown with (NH4_4)2_2MoO4_4-Na2_2SeO3_3 (16mM, 1:1). The dotted lines indicate the grain boundaries. (d) Raman and (e) PL spectra of the as-grown MoSe2_2 film. ~ 30 spectra were obtained from the monolayer MoSe2_2 film shown in (a). (f) The effect of different Na+^{+}:SeO32−_3^{2-}:MoO42−_4^{2-} molar ratios on the CVD growth of MoSe2_2.

Image not extracted

Figure S5. Controlled experiments using different salt precursors. (a, b) A photo and optical images show the repeated growth of MoSe2\mathrm{MoSe}_{2} with (NH4)2MoO4(\mathrm{NH}_{4})_{2}\mathrm{MoO}_{4} only (No Na+\mathrm{Na}^{+} and SeO32−\mathrm{SeO}_{3}^{2-}), and there is no MoSe2\mathrm{MoSe}_{2} was observed after the CVD growth. Inset shows an area of 10×10 μm210 \times10\ \mathrm{\mu m}^{2}. (c, d) A photo and optical images show the repeated growth of MoSe2\mathrm{MoSe}_{2} with (NH4)2MoO4(\mathrm{NH}_{4})_{2}\mathrm{MoO}_{4}-H2SeO3\mathrm{H}_{2}\mathrm{SeO}_{3} (No Na+\mathrm{Na}^{+}), and there is no MoSe2\mathrm{MoSe}_{2} was able to grow the mixed salts. Inset shows an area of 10×10 μm210 \times10\ \mathrm{\mu m}^{2}. (e, f) A photo and optical images show the second growth of monolayer MoSe2\mathrm{MoSe}_{2} film with (NH4)2MoO4(\mathrm{NH}_{4})_{2}\mathrm{MoO}_{4}-Na2SeO3\mathrm{Na}_{2}\mathrm{SeO}_{3} (16 mM16\ \mathrm{mM}, 1:11:1) on a half of 2-inch SiO2/Si\mathrm{SiO}_{2}/\mathrm{Si} wafer, and (f) optical images show the morphology of as-grown monolayer MoSe2\mathrm{MoSe}_{2} film.

Second, it is widely accepted that the Na+\mathrm{Na}^{+} plays vital roles in the growth of TMDCs, which include liquefaction of metal oxides, promoting lateral growth and inducing chalcogen attachment.[17, 20, 23, 42, 43, 44] To validate the importance of Na+\mathrm{Na}^{+}, the MoSe2\mathrm{MoSe}_{2} growth is conducted using salt precursors with/without Na+\mathrm{Na}^{+} at fixed SeO32−\mathrm{SeO}_{3}^{2-} and MoO42−\mathrm{MoO}_{4}^{2-} molar ratio, i.e. (NH4)2MoO4(\mathrm{NH}_{4})_{2}\mathrm{MoO}_{4}-Na2SeO3\mathrm{Na}_{2}\mathrm{SeO}_{3} (16 mM, 1:1) and (NH4)2MoO4(\mathrm{NH}_{4})_{2}\mathrm{MoO}_{4}-H2SeO3\mathrm{H}_{2}\mathrm{SeO}_{3} (16 mM, 1:1). Even with the presence of SeO32−\mathrm{SeO}_{3}^{2-} in the mixed salts, changing the Na+\mathrm{Na}^{+} to H+\mathrm{H}^{+} or reducing the Na+\mathrm{Na}^{+} content leads to poor MoSe2\mathrm{MoSe}_{2} growth (Figure S5-Figure S5 and Figure S6). This further confirms the necessity of Na+\mathrm{Na}^{+} being an indispensable element for the growth of MoSe2\mathrm{MoSe}_{2}. A Na+:MoO42−\mathrm{Na}^{+}:\mathrm{MoO}_{4}^{2-} molar ratio higher than 2 is needed for the successful growth of continuous MoSe2\mathrm{MoSe}_{2} film. This is because the Na+\mathrm{Na}^{+} works better than NH4+\mathrm{NH}_{4}^{+} and H+\mathrm{H}^{+} in stabilizing MoO42−\mathrm{MoO}_{4}^{2-} during the temperature ramping process. Since the use of Na2_2MoO4_4 only lead to an inferior growth, the results above suggest that both Na+^{+} and SeO32−_3^{2-} have a synergistic effect on the enhanced CVD growth of large-area wafer-scale MoSe2_2 film. The effect of different Na+^{+}:SeO32−_3^{2-}:MoO42−_4^{2-} molar ratios on the CVD growth of MoSe2_2 is summarized in Figure 4f.

Image not extracted

Figure S6. Controlled experiments using different Na+^{+} contents. Optical images of MoSe2_2 monolayers grown with Na+^{+}:MoO42−_4^{2-}:SeO32−_3^{2-} molar ratios of (a) 1:1:1 and (b) 0.5:1:1. The molar concentration of MoO42−_4^{2-} and SeO32−_3^{2-} is 16 mM, prepared using a mixture of Na2_2MoO4_4, (NH4_4)2_2MoO4_4 and H2_2SeO3_3.

Besides the above-mentioned reasons, we also notice that the addition of Na2SeO3\mathrm{Na_2SeO_3} to Na2MoO4\mathrm{Na_2MoO_4} results in more uniform precursor coating on SiO2\mathrm{SiO_2}/Si substrates, even after high-temperature annealing (typical CVD process without introducing Se) (Figure S7). This is particularly important as in our previous study on the MoS2\mathrm{MoS_2} growth implied that monolayer films formed only on area covered with densely and uniformly distributed, small Na2MoO4\mathrm{Na_2MoO_4} particles, whereas otherwise on area with low-density, large Na2MoO4\mathrm{Na_2MoO_4} particles.[18] Note that a high Na2SeO3\mathrm{Na_2SeO_3}: Na2MoO4\mathrm{Na_2MoO_4} molar ratio of 2 will lead to the aggregation of mixed salt precursors, forming large particles. In this case, only isolated large monolayer MoSe2\mathrm{MoSe_2} flakes are grown (Figure S2). Hence, careful tuning the molar ratio of the mixed salts is also an important key to the successful growth of continuous monolayer MoSe2\mathrm{MoSe_2} films (Figure 4f).

Image not extracted

Figure S7. Comparison of spin-coated mixed-salt precursors with different Na2_2MoO4_4:Na2_2SeO3_3 molar ratios. The Na2_2MoO4_4:Na2_2SeO3_3 molar ratios are (a) 1:0; (b) 1:0.5; (c) 1:1 and (d) 1:2. In all salt precursors, the Na2_2MoO4_4 is kept as 16 mM. The spin-coating condition is 8000 rpm for 30 s. The first two rows show the morphologies of as-prepared salt precursors on SiO2_2/Si substrates. The third row shows the size and area-density of salt precursors after annealing in a typical CVD process without introducing selenium.

We further calculated the reaction energies for the possible reactions involved during MoSe2\mathrm{MoSe_2} and WTe2\mathrm{WTe_2} growth by using the density functional theory (DFT) method. As shown in Table 1, for a typical growth of MoSe2\mathrm{MoSe_2} with Na2MoO4\mathrm{Na_2MoO_4} only, the reaction energy is -1.1 ev/f.u., Equation (1-1). Increasing the Na2SeO3\mathrm{Na_2SeO_3}/Na2MoO4\mathrm{Na_2MoO_4} ratios from 0.5 to 1 and 2, in Equations (1-2) to (1-3) and (1-4), results in a gradual decrease in the reaction energy from -1.96 to -3.00 and -4.93 ev/f.u., respectively. This implies that the addition of Na2SeO3\mathrm{Na_2SeO_3} is thermodynamically favored for the growth of MoSe2\mathrm{MoSe_2}. For the case of WTe2\mathrm{WTe_2}, a similar trend is observed. The introduction of Na2TeO3\mathrm{Na_2TeO_3} results in a significantly lowered reaction energy from 2.06 ev/f.u. in Equation (2-1) to -0.26 ev/f.u. in Equation (2-2). These results are in consistent to our experimental findings, where the initial poor/limited growth with only the transition metal salts used has improved with the chalcogen salts added, confirming the feasibility of this strategy to the growth of 2D MoSe2\mathrm{MoSe_2} and WTe2\mathrm{WTe_2}.

Possible chemical reactionReaction energy (eV/f.u.)
1-1Na2MoO4+3Se+4H2=MoSe2+Na2Se+4H2O\mathrm{Na}_{2}\mathrm{MoO}_{4} + 3\mathrm{Se} + 4\mathrm{H}_{2} = \mathrm{MoSe}_{2} + \mathrm{Na}_{2}\mathrm{Se} + 4\mathrm{H}_{2}\mathrm{O}-1.1
1-2Na2MoO4+0.5Na2SeO3+3Se+5.5H2=MoSe2+1.5Na2Se+5.5H2O\mathrm{Na}_{2}\mathrm{MoO}_{4} + 0.5\mathrm{Na}_{2}\mathrm{SeO}_{3} + 3\mathrm{Se} + 5.5\mathrm{H}_{2} = \mathrm{MoSe}_{2} + 1.5\mathrm{Na}_{2}\mathrm{Se} + 5.5\mathrm{H}_{2}\mathrm{O}-1.96
1-3Na2MoO4+Na2SeO3+3Se+7H2=MoSe2+2Na2Se+7H2O\mathrm{Na}_{2}\mathrm{MoO}_{4} + \mathrm{Na}_{2}\mathrm{SeO}_{3} + 3\mathrm{Se} + 7\mathrm{H}_{2} = \mathrm{MoSe}_{2} + 2\mathrm{Na}_{2}\mathrm{Se} + 7\mathrm{H}_{2}\mathrm{O}-3.00
1-4Na2MoO4+2Na2SeO3+3Se+10H2=MoSe2+3Na2Se+10H2O\mathrm{Na}_{2}\mathrm{MoO}_{4} + 2\mathrm{Na}_{2}\mathrm{SeO}_{3} + 3\mathrm{Se} + 10\mathrm{H}_{2} = \mathrm{MoSe}_{2} + 3\mathrm{Na}_{2}\mathrm{Se} + 10\mathrm{H}_{2}\mathrm{O}-4.93
2-1Na2WO4+3Te+4H2=WTe2+Na2Te+4H2O\mathrm{Na}_{2}\mathrm{WO}_{4} + 3\mathrm{Te} + 4\mathrm{H}_{2} = \mathrm{WTe}_{2} + \mathrm{Na}_{2}\mathrm{Te} + 4\mathrm{H}_{2}\mathrm{O}2.06
2-2Na2WO4+2Na2TeO3+3Te+10H2=WTe2+3Na2Te+10H2O\mathrm{Na}_{2}\mathrm{WO}_{4} + 2\mathrm{Na}_{2}\mathrm{TeO}_{3} + 3\mathrm{Te} + 10\mathrm{H}_{2} = \mathrm{WTe}_{2} + 3\mathrm{Na}_{2}\mathrm{Te} + 10\mathrm{H}_{2}\mathrm{O}-0.26

Table 1. Possible chemical reactions and corresponding reaction energies for the growth of MoSe2\mathrm{MoSe}_{2} and WTe2\mathrm{WTe}_{2}

CONCLUSIONS

In summary, we demonstrated an enhanced CVD growth of 2D TMD selenides and tellurides using mixed transition metal salts and chalcogen salts. The addition of Na2SeO3\mathrm{Na}_{2}\mathrm{SeO}_{3} to Na2MoO4\mathrm{Na}_{2}\mathrm{MoO}_{4} or (NH4)2MoO4(\mathrm{NH}_{4})_{2}\mathrm{MoO}_{4}, induces a dramatic enhancement in the wafer-scale growth of MoSe2\mathrm{MoSe}_{2}, forming continuous monolayer films with high reproducibility and uniformity at large gain size of 100-250 μm\mu\mathrm{m}. Similarly, high-efficiency growth of WTe2\mathrm{WTe}_{2} is also achieved when mixed salts, Na2WO4\mathrm{Na}_{2}\mathrm{WO}_{4}-Na2TeO3\mathrm{Na}_{2}\mathrm{TeO}_{3} are used as growth precursors. This versatile strategy could also be a useful strategy for the growth of other 2D TMDCs and alloys with heterogeneous chalcogen species.

EXPERIMENTAL SECTION

Growth of 2D TMDCs.

MoSe2\mathrm{MoSe}_{2}. First, mixed Na2MoO4\mathrm{Na}_{2}\mathrm{MoO}_{4}-Na2SeO3\mathrm{Na}_{2}\mathrm{SeO}_{3} solutions with molar ratios of 1:0.5, 1:1 and 1:2 were prepared, respectively. In the mixed salt solutions, the concentration of Na2MoO4\mathrm{Na}_{2}\mathrm{MoO}_{4} was kept 16 mM. Then, the mixed salt solutions were spin-coated onto SiO2\mathrm{SiO}_{2}/Si substrates with a speed of 8000 rpm for 30s. The CVD growth was performed in a 2-inch tube furnace. The growth substrates were placed in the center of tube furnace, while a quartz crucible containing ∼\sim500 mg Se was placed in the upstream at ∼\sim 300 °C during the growth. 200 sccm Ar/H2_{2} (5% H2_{2}) forming gas was introduced as carrier gas. The optimal growth temperature window is 775-850 °C. After CVD growth for 5-10 mins, the tube furnace was cooled down to room temperature in 30 min. To identify the functions of Na (Na+^{+}) and Se (SeO32−_{3}^{2-}) in the enhanced CVD growth of MoSe2\mathrm{MoSe}_{2}, we also preformed controlled CVD growths with Na2MoO4\mathrm{Na}_{2}\mathrm{MoO}_{4}, (NH4)2MoO4(\mathrm{NH}_{4})_{2}\mathrm{MoO}_{4}, (NH4)2MoO4(\mathrm{NH}_{4})_{2}\mathrm{MoO}_{4}-Na2SeO3\mathrm{Na}_{2}\mathrm{SeO}_{3} (1:1) and (NH4)2MoO4(\mathrm{NH}_{4})_{2}\mathrm{MoO}_{4}-H2SeO3\mathrm{H}_{2}\mathrm{SeO}_{3} (1:1), the MoO42−\mathrm{MoO}_{4}^{2-} is 16 mM in all the aqueous solutions.

ReSe2\mathrm{ReSe}_{2}. First, 20 mM mixed NaReO4\mathrm{NaReO}_{4}-Na2SeO3\mathrm{Na}_{2}\mathrm{SeO}_{3} (1:1) aqueous solution was prepared. The mixed salt deposition and CVD processes are similar to the growth of MoSe2\mathrm{MoSe}_{2}. The optimal growth temperature for ReSe2\mathrm{ReSe}_{2} is ∼\sim750 °C.

WTe2\mathrm{WTe}_{2}. First, 20 mM mixed Na2WO4\mathrm{Na}_{2}\mathrm{WO}_{4}-Na2TeO3\mathrm{Na}_{2}\mathrm{TeO}_{3} (1:1) aqueous solution was prepared. Then, the mixed salt solutions were spin-coated onto sapphire substrates with a speed of 5000 rpm for 30s. The growth substrates were placed in the center of the 2-inch tube furnace with a new quartz tube. A quartz crucible containing ∼\sim500 mg Te was placed in the upstream at ∼\sim 550 °C during growth. 100 sccm Ar/H2_{2} (5% H2_{2}) forming gas was introduced as carrier gas. The optimal growth temperature window is 775-825 °C. After CVD growth for 5 mins, the tube furnace was cooled down to room temperature in 30 min.

Characterization of 2D TMDCs.

Raman and PL. The micro-Raman/PL was performed using a laser confocal microscope (inVia, Renishaw). The 532-nm excitation laser was focused on the sample surface with a 100×100 \times objective lens. Then, Raman/PL signals from the TMDC samples were detected by an electron multiplying CCD detector (Andor) through a grating with 1800 grooves/mm for Raman and 300 grooves/mm for PL. The laser spot size was about 1 μm1\ \mu\mathrm{m} in diameter. Raman and PL mapping were conducted on the large MoSe2\mathrm{MoSe}_2 monolayers with a step of 0.5 μm0.5\ \mu\mathrm{m}.

AFM. The AFM observations were performed in tapping mode by Asylum MFP-3D origin.

STEM. STEM images of MoSe2\mathrm{MoSe}_2 monolayer were acquired by using JEOL 2100F microscope equipped with dodecaple correctors and the cold field emission gun operating at 60 kV. The probe current was about 25-30 pA. The convergence semiangle was 35 mrad and the inner acquisition semiangle was 79 mrad.

Device fabrication and test.

Device fabrication. For the large MoSe2\mathrm{MoSe}_2 monolayers transferred on heavily doped silicon substrates with 285-nm-thick SiO2\mathrm{SiO}_2 layer, a layer of photoresist (OFPR-800LB, TOK) was first spin-coated at a speed of 5000 rpm for 30 s. Then, the substrates were baked at 100 °C for 5 mins. A standard LED photolithography process was conducted to define the channel shape (protected by photoresist after development). After developing in NMD-3 (TOK) and rinse with DI water, the surrounding exposed MoSe2_2 monolayers were etched with oxygen plasma.

Next, a second LED photolithography was conducted to define the electrode patterns. Tri-layer of Cr/Pd/Au (1/10/50 nm) was deposited as contacts via e-beam deposition. The final MoSe2_2-FETs have channel length of ∼5\sim5 μ\mum and with of ∼20\sim20 μ\mum (Figure S3). Similar fabrication process was also conducted on the transferred ReSe2_2 and WTe2_2 without the etching procedure. For ReS2_2- and WTe2_2-FETs, bi-layer of Cr/Au (1/50 nm) were deposited as contacts.

Measurement of TMDC-based FETs. To test the transport properties of MoSe2_2-FETs, the devices were loaded in a vacuum chamber with a pressure of ∼2×10−3\sim2 \times10^{-3} Pa. The backgate bias (VgsV_{\mathrm{gs}}) was scanned forward from -10 V to 50 V and backward from 50 V to -10 V with a step of 1 V, the source-drain bias (VdsV_{\mathrm{ds}}) is 2 V. For the transport curves plotted in Figure 2j, the y-axis was normalized to conductivity using the channel current and device dimensions. For the WTe2_2-FETs, the backgate bias (VgsV_{\mathrm{gs}}) was scanned forward from -30 V to 30 V and backward from 30 V to -30 V with a step of 1 V, the source-drain bias (VdsV_{\mathrm{ds}}) is 1 V.

Density functional theory (DFT) calculation.

The reaction energies were evaluated using the DFT method within the generalized gradient approximation of the Perdew, Burke, and Ernzerhof functional as implemented in the Vienna ab initio simulation package.[45, 46] Electron−ion interactions were described using projector-augmented wave pseudopotentials.[47] A plane-wave kinetic-energy cutoff of 600 eV and a k-spacing of 0.2 Å−1^{-1} in reciprocal space were used to ensure that the energy converged to better than 1 meV/atom. All of the crystal structures were obtained from the Materials Project database.[48]

ASSOCIATED CONTENT

Supporting Information.

This material is available free of charge via the Internet at http://pubs.acs.org.

The Supporting Information include: (i) schematic illustration of mixed-salt CVD process, (ii) characterization of as-grown 2D MoSe2\mathrm{MoSe}_{2} and ReSe2\mathrm{ReSe}_{2}, (iii) characterization of MoSe2\mathrm{MoSe}_{2}-FETs, (iv) calculated energy of chemicals.

AUTHOR INFORMATION

Corresponding Authors

S. Li: [email protected]

T. Taniguchi: [email protected]

ORCID

Shisheng Li: 0000-0001-9301-5559

Yung-Chang Lin: 0000-0002-3968-7239

Jinhua Hong: 0000-0002-6406-1780

Bo Gao: 0000-0003-1183-656X

Hong En Lim: 0000-0003-0347-8897

Xu Yang: 0000-0001-8195-5850

Song Liu: 0000-0003-3390-7795

Yoshitaka Tateyama: 0000-0002-5532-6134

Yoshiki Sakuma: 0000-0001-68047217

Kazuhito Tsukagoshi: 0000-0001-9710-2692

Kazu Suenaga: 0000-0002-6107-1123

Takaaki Taniguchi: 0000-0002-8460-5431

Notes

The authors declare no competing financial interests.

Acknowledgment

S.L. acknowledges the support from JSPS-KAKENHI (19K15399, 21K04839). T.T. acknowledges the support from JSPS-KAKENHI (17K19187). Y.-C.L. and K.S. acknowledge support from the JST-CREST (JPMJCR20B1, JPMJCR20B5, JPMJCR1993), JSPS-KAKENHI (18K14119), JSPS A3 Foresight Program, and Kazato Research Encouragement Prize. Y.S. acknowledges the support from JSPS-KAKENHI (17H03241). H.E.L. acknowledges the support from JSPS-KAKENHI (19K15393, 21K14498). B.G. and Y.T. thank the support by MEXT as “Program for Promoting Researches on the Supercomputer Fugaku (Fugaku Battery & Fuel Cell Project), Grant JPMXP1020200301, and the supercomputer at NIMS. S.L. acknowledges all staff members of the Nanofabrication Group at NIMS for their support.

Mixed Salt CVD_SI_210824

Energy (eV/f.u.)Energy (eV/f.u.)
MoSe2\mathrm{MoSe}_{2}-19.973WTe2\mathrm{WTe}_{2}-19.575
Na2MoO4\mathrm{Na}_{2}\mathrm{MoO}_{4}-47.597Na2WO4\mathrm{Na}_{2}\mathrm{WO}_{4}-50.638
Na2SeO3\mathrm{Na}_{2}\mathrm{SeO}_{3}-29.870Na2TeO3\mathrm{Na}_{2}\mathrm{TeO}_{3}-29.831
Na2Se\mathrm{Na}_{2}\mathrm{Se}-9.387Na2Te\mathrm{Na}_{2}\mathrm{Te}-8.607
Se\mathrm{Se}-3.506Te\mathrm{Te}-3.142
H2\mathrm{H}_{2}-6.773H2O\mathrm{H}_{2}\mathrm{O}-14.229

Table S1. Calculated energy of chemicals

References

  1. [1]Fiori, G.; Bonaccorso, F.; Iannaccone, G.; Palacios, T.; Neumaier, D.; Seabaugh, A.; Banerjee, S. K.; Colombo, L., Electronics Based on Two-Dimensional Materials. Nat. Nanotechnol. 2014, 9, 768-779.DOI
  2. [2]Gong, C.; Zhang, Y.; Chen, W.; Chu, J.; Lei, T.; Pu, J.; Dai, L.; Wu, C.; Cheng, Y.; Zhai, T., Electronic and Optoelectronic Applications Based on 2D Novel Anisotropic Yransition Metal Dichalcogenides. Adv. Sci. 2017, 4, 1700231.DOI
  3. [3]Su, S.-K.; Chuu, C.-P.; Li, M.-Y.; Cheng, C.-C.; Wong, H.-S. P.; Li, L.-J., Layered Semiconducting 2D Materials for Future Transistor Applications. Small Structures, 2021, 2, 2000103.DOI
  4. [4]Shi, J.; Huan, Y.; Zhao, X.; Yang, P.; Hong, M.; Xie, C.; Pennycook, S.; Zhang, Y., Two-Dimensional Metallic Vanadium Ditelluride as a High-Performance Electrode Material. ACS Nano 2021, 15, 1858-1868.DOI
  5. [5]Zhang, Z.; Gong, Y.; Zou, X.; Liu, P.; Yang, P.; Shi, J.; Zhao, L.; Zhang, Q.; Gu, L.; Zhang, Y., Epitaxial Growth of Two-Dimensional Metal–Semiconductor Transition-Metal Dichalcogenide Vertical Stacks (VSe₂/MX₂) and Their Band Alignments. ACS Nano 2018, 13, 885-893.
  6. [6]Mleczko, M. J.; Xu, R. L.; Okabe, K.; Kuo, H.-H.; Fisher, I. R.; Wong, H.-S. P.; Nishi, Y.; Pop, E., High Current Density and Low Thermal Conductivity of Atomically Thin Semimetallic WTe₂. ACS Nano 2016, 10, 7507-7514.DOI
  7. [7]Lee, C.-S.; Oh, S. J.; Heo, H.; Seo, S.-Y.; Kim, J.; Kim, Y. H.; Kim, D.; Ngome Okello, O. F.; Shin, H.; Sung, J. H., Epitaxial van der Waals Contacts Between Transition-Metal Dichalcogenide Monolayer Polymorphs. Nano Lett. 2019, 19, 1814-1820.DOI
  8. [8]Tan, J.; Li, S.; Liu, B.; Cheng, H.-M., Structure, Preparation, and Applications of 2D Material-Based Metal–Semiconductor Heterostructures. Small Structures 2021, 2, 2000093.
  9. [9]Kang, K.; Xie, S.; Huang, L.; Han, Y.; Huang, P. Y.; Mak, K. F.; Kim, C.-J.; Muller, D.; Park, J., High-Mobility Three-Atom-Thick Semiconducting Films with Wafer-Scale Homogeneity. Nature 2015, 520, 656-660.DOI
  10. [10]Wang, D.; Luo, F.; Lu, M.; Xie, X.; Huang, L.; Huang, W., Chemical Vapor Transport Reactions for Synthesizing Layered Materials and Their 2D Counterparts. Small 2019, 15, 1804404.DOI
  11. [11]Lee, Y. H.; Zhang, X. Q.; Zhang, W.; Chang, M. T.; Lin, C. T.; Chang, K. D.; Yu, Y. C.; Wang, J. T. W.; Chang, C. S.; Li, L. J., Synthesis of Large-Area MoS₂ Atomic Layers with Chemical Vapor Deposition. Adv. Mater. 2012, 24, 2320-2325.DOI
  12. [12]Shi, Y.; Li, H.; Li, L.-J., Recent Advances in Controlled Synthesis of Two-Dimensional Transition Metal Dichalcogenides via Vapour Deposition Techniques. Chem. Soc. Rev. 2015, 44, 2744-2756.DOI
  13. [13]Huang, J.-K.; Pu, J.; Hsu, C.-L.; Chiu, M.-H.; Juang, Z.-Y.; Chang, Y.-H.; Chang, W.-H.; Iwasa, Y.; Takenobu, T.; Li, L.-J., Large-Area Synthesis of Highly Crystalline WSe₂ Monolayers and Device Applications. ACS Nano 2014, 8, 923-930.
  14. [14]Li, S.; Wang, S.; Tang, D.-M.; Zhao, W.; Xu, H.; Chu, L.; Bando, Y.; Golberg, D.; Eda, G., Halide-Assisted Atmospheric Pressure Growth of Large WSe₂ and WS₂ Monolayer Crystals. Appl. Mater. Today 2015, 1, 60-66.DOI
  15. [15]Zhou, J.; Lin, J.; Huang, X.; Zhou, Y.; Chen, Y.; Xia, J.; Wang, H.; Xie, Y.; Yu, H.; Lei, J., A Library of Atomically Thin Metal Chalcogenides. Nature 2018, 556, 355-359.DOI
  16. [16]Liu, C.; Xu, X.; Qiu, L.; Wu, M.; Qiao, R.; Wang, L.; Wang, J.; Niu, J.; Liang, J.; Zhou, X., Kinetic Modulation of Graphene Growth by Fluorine Through Spatially Confined Decomposition of Metal Fluorides. Nat. Chem. 2019, 11, 730-736.DOI
  17. [17]Li, S.; Lin, Y.-C.; Zhao, W.; Wu, J.; Wang, Z.; Hu, Z.; Shen, Y.; Tang, D.-M.; Wang, J.; Zhang, Q., Vapour–Liquid–Solid Growth of Monolayer MoS₂ Nanoribbons. Nat. Mater. 2018, 17, 535-542.DOI
  18. [18]Li, S.; Lin, Y.-C.; Liu, X.-Y.; Hu, Z.; Wu, J.; Nakajima, H.; Liu, S.; Okazaki, T.; Chen, W.; Minari, T., Wafer-Scale and Deterministic Patterned Growth of Monolayer MoS₂ via Vapor–Liquid–Solid Method. Nanoscale 2019, 11, 16122-16129.DOI
  19. [19]Liu, H.; Qi, G.; Tang, C.; Chen, M.; Chen, Y.; Shu, Z.; Xiang, H.; Jin, Y.; Wang, S.; Li, H., Growth of Large-Area Homogeneous Monolayer Transition-Metal Disulfides via a Molten Liquid Intermediate Process. ACS Appl. Mater. & Interfaces 2020, 12, 13174-13181.DOI
  20. [20]Chang, M.-C.; Ho, P.-H.; Tseng, M.-F.; Lin, F.-Y.; Hou, C.-H.; Lin, I.-K.; Wang, H.; Huang, P.-P.; Chiang, C.-H.; Yang, Y.-C., Fast Growth of Large-Grain and Continuous MoS₂ Films Through a Self-Capping Vapor-Liquid-Solid Method. Nat. Commun. 2020, 11, 3682.DOI
  21. [21]Zuo, Y.; Yu, W.; Liu, C.; Cheng, X.; Qiao, R.; Liang, J.; Zhou, X.; Wang, J.; Wu, M.; Zhao, Y., Optical Fibres with Embedded Two-Dimensional Materials for Ultrahigh Nonlinearity. Nat. Nanotechnol. 2020, 15, 987-991.DOI
  22. [22]Li, S.; Hong, J.; Gao, B.; Lin, Y. C.; Lim, H. E.; Lu, X.; Wu, J.; Liu, S.; Tateyama, Y.; Sakuma, Y., Tunable Doping of Rhenium and Vanadium into Transition Metal Dichalcogenides for Two-Dimensional Electronics. Adv. Sci. 2021, 8, 2004438.DOI
  23. [23]Cai, Z.; Lai, Y.; Zhao, S.; Zhang, R.; Tan, J.; Feng, S.; Zou, J.; Tang, L.; Lin, J.; Liu, B., Dissolution-Precipitation Growth of Uniform and Clean Two Dimensional Transition Metal Dichalcogenides. Nat. Sci. Rev. 2021, 8, nwaal15.arxiv.org/abs/2007.06917
  24. [24]Gong, Y.; Lin, Z.; Ye, G.; Shi, G.; Feng, S.; Lei, Y.; Elias, A. L.; Perea-Lopez, N.; Vajtai, R.; Terrones, H., Tellurium-Assisted Low-Temperature Synthesis of MoS₂ and WS₂ Monolayers. ACS Nano 2015, 9, 11658-11666.DOI
  25. [25]Cui, F.; Wang, C.; Li, X.; Wang, G.; Liu, K.; Yang, Z.; Feng, Q.; Liang, X.; Zhang, Z.; Liu, S., Tellurium-Assisted Epitaxial Growth of Large-area, Highly Crystalline ReS₂ Atomic Layers on Mica Substrate. Adv. Mater. 2016, 28, 5019-5024.DOI
  26. [26]Tonndorf, P.; Schmidt, R.; Böttger, P.; Zhang, X.; Börner, J.; Liebig, A.; Albrecht, M.; Kloc, C.; Gordan, O.; Zahn, D. R., Photoluminescence Emission and Raman Response of Monolayer MoS₂, MoSe₂, and WSe₂. Opt. Express 2013, 21, 4908-4916.DOI
  27. [27]Liu, Z.; Amani, M.; Najmaei, S.; Xu, Q.; Zou, X.; Zhou, W.; Yu, T.; Qiu, C.; Birdwell, A. G.; Crowne, F. J., Strain and Structure Heterogeneity in MoS₂ Atomic Layers Grown by Chemical Vapour Deposition. Nat. Commun. 2014, 5, 5246.DOI
  28. [28]Yang, S.; Chen, Y.; Jiang, C., Strain Engineering of Two-Dimensional Materials: Methods, Properties, and Applications. InfoMat 2021, 3, 397-420.DOI
  29. [29]Wang, X.; Gong, Y.; Shi, G.; Chow, W. L.; Keyshar, K.; Ye, G.; Vajtai, R.; Lou, J.; Liu, Z.; Ringe, E., Chemical Vapor Deposition Growth of Crystalline Monolayer MoSe₂. ACS Nano 2014, 8, 5125-5131.DOI
  30. [30]Han, H.-V.; Lu, A.-Y.; Lu, L.-S.; Huang, J.-K.; Li, H.; Hsu, C.-L.; Lin, Y.-C.; Chiu, M.-H.; Suenaga, K.; Chu, C.-W., Photoluminescence Enhancement and Structure Repairing of Monolayer MoSe₂ by Hydrohalic Acid Treatment. ACS Nano 2016, 10, 1454-1461.DOI
  31. [31]Chen, M.-W.; Ovchinnikov, D.; Lazar, S.; Pizzocchero, M.; Whitwick, M. B.; Surrente, A.; Baranowski, M.; Sanchez, O. L.; Gillet, P.; Plochocka, P., Highly Oriented Atomically Thin Ambipolar MoSe₂ Grown by Molecular Beam Epitaxy. ACS Nano 2017, 11, 6355-6361.DOI
  32. [32]Meng, Y.; Ling, C.; Xin, R.; Wang, P.; Song, Y.; Bu, H.; Gao, S.; Wang, X.; Song, F.; Wang, J., Repairing Atomic Vacancies in Single-Layer MoSe₂ Field-Effect Transistor and Its Defect Dynamics. npj Quantum Mater. 2017, 2, 16.arxiv.org/abs/1601.05534
  33. [33]Li, Y.; Zhang, K.; Wang, F.; Feng, Y.; Li, Y.; Han, Y.; Tang, D.; Zhang, B., Scalable Synthesis of Highly Crystalline MoSe₂ and Its Ambipolar Behavior. ACS Appl. Mater. & Interfaces 2017, 9, 36009-36016.DOI
  34. [34]Chen, X.; Hu, P.; Song, K.; Wang, X.; Zuo, C.; Yang, R.; Wang, J., CVD Growth of Large-Scale Hexagon-Like Shaped MoSe₂ Monolayers with Sawtooth Edge. Chem. Phys. Lett. 2019, 733, 136663.
  35. [35]Somvanshi, D.; Ber, E.; Bailey, C. S.; Pop, E.; Yalon, E., Improved Current Density and Contact Resistance in Bilayer MoSe₂ Field Effect Transistors by AlOₓ Capping. ACS Appl. Mater. & Interfaces 2020, 12, 36355-36361.DOI
  36. [36]Kim, M.; Seo, J.; Kim, J.; Moon, J. S.; Lee, J.; Kim, J.-H.; Kang, J.; Park, H., High-Crystalline Monolayer Transition Metal Dichalcogenides Films for Wafer-Scale Electronics. ACS Nano 2021, 15, 3038-3046.DOI
  37. [37]Chen, Z.; Liu, H.; Chen, X.; Chu, G.; Chu, S.; Zhang, H., Wafer-Size and Single-Crystal MoSe₂ Atomically Thin Films Grown on GaN Dubstrate for Light Emission and Harvesting. ACS Appl. Mater. Interfaces 2016, 8, 20267-20273.DOI
  38. [38]Li, J.; Yan, W.; Lv, Y.; Leng, J.; Zhang, D.; Coileáin, C. Ó.; Cullen, C. P.; Stimpel-Lindner, T.; Duesberg, G. S.; Cho, J., Sub-Millimeter Size High Mobility Single Crystal MoSe₂ Monolayers Synthesized by NaCl-Assisted Chemical Vapor Deposition. RSC Adv. 2020, 10, 1580-1587.DOI
  39. [39]Li, N.; Wang, Q.; Shen, C.; Wei, Z.; Yu, H.; Zhao, J.; Lu, X.; Wang, G.; He, C.; Xie, L., Large-Scale Flexible and Transparent Electronics Based on Monolayer Molybdenum Disulfide Field-Effect Transistors. Nat. Electron. 2020, 3, 711-717.DOI
  40. [40]Zhou, Z.; Xu, T.; Zhang, C.; Li, S.; Xu, J.; Sun, L.; Gao, L., Enhancing Stability by Tuning Element Ratio in 2D Transition Metal Chalcogenides. Nano Res. 2021, 14, 1704-1710.DOI
  41. [41]Li, J.; Cheng, S.; Liu, Z.; Zhang, W.; Chang, H., Centimeter-Scale, Large-Area, Few-Layer 1T′-WTe₂ Films by Chemical Vapor Deposition and Its Long-Term Stability in Ambient Condition. J. Phys. Chem. C 2018, 122, 7005-7012.DOI
  42. [42]Yang, P.; Zou, X.; Zhang, Z.; Hong, M.; Shi, J.; Chen, S.; Shu, J.; Zhao, L.; Jiang, S.; Zhou, X., Batch Production of 6-Inch Uniform Monolayer Molybdenum Disulfide Catalyzed by Sodium in Glass. Nat. Commun. 2018, 9, 979.DOI
  43. [43]Xie, C.; Yang, P.; Huan, Y.; Cui, F.; Zhang, Y., Roles of Salts in the Chemical Vapor Deposition Synthesis of Two-Dimensional Transition Metal Chalcogenides. Dalton Trans. 2020, 49, 10319-10327.DOI
  44. [44]Kim, H.; Ovchinnikov, D.; Deiana, D.; Unuchek, D.; Kis, A., Suppressing Nucleation in Metal–Organic Chemical Vapor Deposition of MoS₂ Monolayers by Alkali Metal Halides. Nano Lett. 2017, 17, 5056-5063.DOI
  45. [45]Perdew, J. P.; Burke, K.; Ernzerhof, M., Generalized gradient approximation made simple. Phys. Rev. Lett. 1996, 77, 3865.pubmed.ncbi.nlm.nih.gov/10062328
  46. [46]Kresse, G.; Joubert, D., From ultrasoft pseudopotentials to the projector augmented-wave method. Phys. Rev. B 1999, 59, 1758.DOI
  47. [47]Blöchl, P. E., Projector augmented-wave method. Phy. Rev. B 1994, 50, 17953.pubmed.ncbi.nlm.nih.gov/9976227
  48. [48]Jain, A.; Ong, S. P.; Hautier, G.; Chen, W.; Richards, W. D.; Dacek, S.; Cholia, S.; Gunter, D.; Skinner, D.; Ceder, G., Commentary: The Materials Project: A materials genome approach to accelerating materials innovation. APL Mater. 2013, 1, 011002.DOI

Paper details

vlnc:W_u53b4cp2
Version
v1 · latest
Published
Fresh — added to the Hub within the last 30 days
Added
License
CC BY 4.0
Usage

views · 0

downloads · 0

A view counts once per browser per day, a download each time the PDF is requested.

  • Physics and Astronomy

Not recorded for this paper

View statement
Looking for related papers…
Contents