Bidirectional Optimization onto Thermoelectric Performance via Hydrostatic-Pressure in Chalcopyrite AgXTe2 (X=In, Ga)

Abstract

Pressure tuning has emerged as a powerful strategy for manipulating the thermoelectric properties of materials by inducing structural and electronic modifications. Herein, we systematically investigate the transport properties and thermoelectric performance concerning lattice distortions induced by hydrostatic pressure in Ag-based chalcopyrite AgXTe2 (X=In, Ga). The findings reveal that the lattice distortion in AgXTe2 exhibits distinct behaviors under lattice compression, diverging from trends observed at ambient pressure. Importantly, the hydrostatic pressure breaks the phenomenally negative correlation between thermal conductivity and lattice distortion. Pressure-induced softening of low-frequency acoustic phonons broadens the low-energy phonon spectrum, enhancing interactions between acoustic and optical phonons. Such broadening substantially increases the number of available three-phonon scattering channels, resulting in a marked reduction in thermal conductivity. Meanwhile, we establish a macroscopic connection between metavalent bonding and anharmonicity, providing an indirect explanation for lattice anharmonicity through pressure-driven transferred charge. Additionally, the applied pressure achieves a notable net increase in the power factor despite the strong coupling of electrical transport parameters, which underscores the potential for bidirectional optimization of transport properties in AgXTe2. As a result, the maximum ZT value of AgInTe2 is nearly doubled, demonstrating that pressure modulation is a powerful strategy for enhancing thermoelectric performance. Our work not only establishes the link between pressure, lattice dynamics, and thermoelectric properties within chalcopyrite AgXTe2, but also inspires the exploration of pressure-related optimization strategies for conventional thermoelectric materials.

INTRODUCTION

Thermoelectric (TE) materials belong to the distinctive category of functional materials capable of interconverting thermal and electrical energies [1, 2, 3, 4]. The dimensionless figure of merit ZT=S2σT/(κe+κL)ZT=S^{2}\sigma T/(\kappa_{\mathrm{e}}+\kappa_{\mathrm{L}}), where SS, σ\sigma, κe\kappa_{\mathrm{e}}, and κL\kappa_{\mathrm{L}} represent the Seebeck coefficient, electrical conductivity, electronic and lattice thermal conductivity, respectively, is used to evaluate thermoelectric properties [2, 5, 6]. An ideal thermoelectric material should simultaneously exhibit several key characteristics: high electrical conductivity to minimize internal energy dissipation, a substantial Seebeck coefficient to generate significant voltage, and low thermal conductivity to maintain a robust temperature gradient. The intricate coupling among these parameters, however, poses a formidable challenge to the optimization of ZTZT [7, 8, 9].

A promising strategy to address this challenge is the application of hydrostatic pressure [10, 11]. The application of external pressure can induce significant changes in the crystal and electronic structures of materials, which may lead to the decoupling of the fundamental physical parameters, including SS, σ\sigma, κe\kappa_{\mathrm{e}}, and κL\kappa_{\mathrm{L}}, thereby enabling the simultaneous optimization of electronic and lattice transport properties, a phenomenon that has emerged as a critical factor in modulating the thermoelectric material properties, as recent scientific advancements have evidenced [12, 13]. Experimental investigations have revealed that in the pressure range up to 30 GPa, the thermal conductivity of BAs shows an anomalous trend of increasing and then decreasing with pressure, and this complex behavior is attributed to the competing relationship between the three-phonon and four-phonon processes dominating the scattering under the influence of pressure [14]. Moreover, studies have demonstrated that the application of pressure to SnSe induces the formation of additional conduction band valleys, thereby enhancing band degeneracy and consequently improving its thermoelectric properties [15, 16]. These findings demonstrate the potential of pressure in enhancing the thermoelectric performance of materials by modifying their crystallographic and electronic configurations.

Diamond-like materials with low-symmetry structures have garnered significant interest in the fields of electronics and optoelectronics, owing to their broad electronic band gaps [17, 18, 19, 20]. It is noteworthy that these materials also exhibit remarkable thermoelectric properties, as exemplified by ternary chalcopyrite [21, 22, 23]. Experimental results have demonstrated that the incorporation of Ag and Ga into the Cu1−xAgxInTe2\mathrm{Cu}_{1-x}\mathrm{Ag}_{x}\mathrm{InTe}_{2} and (Cu1−xAgx)(In1−yGay)Te2(\mathrm{Cu}_{1-x}\mathrm{Ag}_{x})(\mathrm{In}_{1-y}\mathrm{Ga}_{y})\mathrm{Te}_{2} systems have resulted in a maximum ZTZT value of 1.6, representing the highest value reported to date [24, 25, 26]. This exceptional performance has been attributed to the unique electronic property of chalcopyrite compounds, which exhibit full conformity to the recently defined metavalent bonding region, characterized by pronounced anharmonicity [27]. Further investigation revealed that the high performance observed in chalcopyrite compounds AgGaTe2\mathrm{AgGaTe}_{2} was attributed to strong phonon scattering caused by distorted Ag tetrahedra, a consequence of weak sd3sd^{3} orbital hybridization in Ag atoms [28]. These insights have deepened our understanding of chalcopyrite compounds and have led to a growing interest in the structure of diamondoid chalcopyrites. At present, anomalous thermal transport of chalcopyrite structures at high pressures has been reported. [22, 29, 30, 31] For example, a negative correlation between pressure and thermal conductivity has been observed in CuInTe2\mathrm{CuInTe}_{2} [30, 31]. While these findings provide valuable insights, the microscopic mechanisms underlying the anomalous thermal transport behavior under pressure remain inadequately understood, and there is a need for further comprehensive and systematic studies to uncover the underlying physical principles.

In this study, we comprehensively investigated the thermal/electron transport and thermoelectric properties under the lattice distortions caused by hydrostatic pressure in Ag-based chalcopyrites AgXTe2\mathrm{AgXTe}_{2} (X=In, Ga). This study reveals lattice distortion in AgXTe2\mathrm{AgXTe}_{2} at ambient pressure, suggesting a high phonon scattering rate due to the structural complexity. Under applied pressure, the distortion in AgInTe2\mathrm{AgInTe}_{2} remains relatively constant, while that of AgGaTe2\mathrm{AgGaTe}_{2} increases monotonically. We calculated the lattice thermal conductivity of both compounds under various pressures and found that the correlation between lattice distortion and thermal conductivity is decoupled at pressures. Further analysis reveals a significant increase in the three-phonon scattering phase space for AgInTe2\mathrm{AgInTe}_{2} under pressure, which is identified as the primary driver of the substantial change in κL\kappa_{\mathrm{L}}. Moreover, the impact of pressure on electronic transport properties was investigated, demonstrating a considerable enhancement of carrier mobility considering three dominant scattering mechanisms. Notably, a positive correlation between charge transfer and anharmonicity is observed within the compounds, with pressure-induced charge transfer leading to a substantial increase in anharmonicity. These findings suggest that the application of pressure can effectively enhance the overall thermoelectric performance of chalcopyrite AgXTe2\mathrm{AgXTe}_{2} (X=In, Ga) by simultaneously optimizing both thermal and electronic transport properties.

COMPUTATIONAL METHODS

Density-function theory calculation

Based on the framework of density functional theory (DFT), first-principles calculations are performed in the VASP software package using the projector augmented wave (PAW) method [32, 33, 34]. We used the generalized gradient approximation (GGA) of the Perdew-Burke-Ernzerhof (PBE) functional to describe the exchange-correlation interaction [35, 36]. A plane-wave cut-off of 600 eV was used in all the calculations. We considered the AgXTe2\mathrm{AgXTe}_{2} (X=In, Ga) compound with a chalcopyrite-type structure, which has a unit cell containing 4 Ag atoms, 4 In (or Ga) atoms, and 8 Te atoms. The projector augmented wave pseudopotentials were used to treat the Ag (4d105s14d^{10}5s^{1}), In (5s25p15s^{2}5p^{1}), Ga (4s24p14s^{2}4p^{1}) and Te (5s25p45s^{2}5p^{4}) shells as valence states. The geometry optimization and phonon calculations were performed with the total energy and forces convergence criteria of 10−810^{-8} eV and 10−610^{-6} eV/Å respectively. To overcome the severe band gap underestimation of the PBE functional for semiconductor materials, we employed the HSE06 hybrid functional to investigate the band gap and electronic band structure of AgGaTe2\mathrm{AgGaTe}_{2} [37, 38]. The static dielectric constant of AgGaTe2\mathrm{AgGaTe}_{2} was obtained from the hybrid functional calculations at a dense 8×8×88\times8\times8 kk-point mesh.

Interatomic force constants and thermal transport

The relaxed crystal structure was then used in the phonon calculations, which were carried out by the Phonopy software package [39]. The second-order force constant and the phonon dispersion were obtained using a 2×2×12\times2\times1 supercell with 6×6×66\times6\times6 kk-grid. To extract the third-order interatomic force constant, we used the Thirdorder software package and generated 780 displacement cells by considering 9 adjacent atoms [40]. The lattice thermal conductivity is calculated by iteratively solving the phonon Boltzmann transport equation as implemented in the ShengBTE package with the 12×12×1212\times12\times12 qq-grid [41]. The κL\kappa_{\mathrm{L}} tensor can be expressed as

κLαβ(T)=1NΩ∑q,jCq,j(T)vq,jαvq,jβτq,j(T)(1)\kappa_{\mathrm{L}}^{\alpha\beta}(T)=\frac{1}{N\Omega}\sum_{\mathbf{q},j}C_{\mathbf{q},j}(T)v_{\mathbf{q},j}^{\alpha}v_{\mathbf{q},j}^{\beta}\tau_{\mathbf{q},j}(T) \tag*{(1)}

where NN, Ω\Omega, Cq,j(T)C_{\mathbf{q},j}(T), and vq,jv_{\mathbf{q},j} represent the total number of sampling, the volume system, specific heat capacity, and group velocity, respectively. The τq,j\tau_{\mathbf{q},j} is defined as the inverse of the scattering rate. Specifically, the three-phonon scattering probability Γλλ′λ′′±\Gamma^{\pm}_{\lambda\lambda'\lambda''} can be expressed as,

Γλλ′λ′′±=ℏπ8N{2(fλ′−fλ′′)fλ′+fλ′′+1}×δ(ωλ±ωλ′−ωλ′′)ωλωλ′ωλ′′∣Vλλ′λ′′±∣2(2)\Gamma^{\pm}_{\lambda\lambda'\lambda''}=\frac{\hbar\pi}{8N}\left\{\frac{2(f_{\lambda'}-f_{\lambda''})}{f_{\lambda'}+f_{\lambda''}+1}\right\}\times\frac{\delta(\omega_{\lambda}\pm\omega_{\lambda'}-\omega_{\lambda''})}{\omega_{\lambda}\omega_{\lambda'}\omega_{\lambda''}}\left|V^{\pm}_{\lambda\lambda'\lambda''}\right|^{2} \tag*{(2)}
CompoundPressure (GPa)a/ba/b (Å)cc (Å)Ag-Te (Å)In/Ga-Te (Å)η\eta
AgInTe2_206.5713.022.812.860.019
46.3912.642.722.790.020
AgGaTe2_206.4112.342.802.680.073
3.86.2611.992.732.620.083

Table 1. Structural parameters of AgInTe2_2 and AgGaTe2_2 under different pressures: lattice constants (a/ba/b, cc), bond lengths (Ag-Te, In/Ga-Te), tetragonal distortion (η\eta).

where the upper (lower) row in curly brackets goes with the + (-) sign for absorption (emission) processes, respectively. The scattering matrix elements Vλλ′λ′′±V^{\pm}_{\lambda\lambda'\lambda''} depend on the third order interatomic force constants (IFCs).

Electronic properties and electron-phonon coupling

To evaluate the electrical transport properties, we utilized the AMSET code [42], which allowed for accurate calculations of electron scattering processes and relaxation times. The differential scattering rate for transitions from an initial electronic state Ψnk\Psi_{n\mathbf{k}} to final states Ψmk+q\Psi_{m\mathbf{k}+\mathbf{q}}, accounting for both inelastic and elastic scattering events, is computed using the following expressions. For inelastic scattering processes, such as polar optical phonon (POP) interactions, the scattering rate is given by:

τnk→mk+q−1=2πℏ∣gnm(k,q)∣2[(npo+1−fmk+q)δ(εnk−εmk+q−ℏωpo)+(npo+fmk+q)δ(εnk−εmk+q+ℏωpo)](3)\tau^{-1}_{n\mathbf{k}\to m\mathbf{k}+\mathbf{q}} = \frac{2\pi}{\hbar} \lvert g_{nm}(\mathbf{k},\mathbf{q}) \rvert^2 \left[(n_{\mathrm{po}}+1-f_{m\mathbf{k}+\mathbf{q}})\delta(\varepsilon_{n\mathbf{k}}-\varepsilon_{m\mathbf{k}+\mathbf{q}}-\hbar\omega_{\mathrm{po}})+(n_{\mathrm{po}}+f_{m\mathbf{k}+\mathbf{q}})\delta(\varepsilon_{n\mathbf{k}}-\varepsilon_{m\mathbf{k}+\mathbf{q}}+\hbar\omega_{\mathrm{po}})\right] \tag*{(3)}

Here, npon_{\mathrm{po}} denotes the phonon occupation number, fmk+qf_{m\mathbf{k}+\mathbf{q}} represents the Fermi-Dirac distribution function, and ωpo\omega_{\mathrm{po}} is the polar optical phonon frequency. The delta functions enforce energy conservation for phonon absorption and emission processes. The εnk\varepsilon_{n\mathbf{k}} and εmk+q\varepsilon_{m\mathbf{k}+\mathbf{q}} represent the energies of the initial and final electronic states, respectively.

For elastic scattering, such as acoustic deformation potential (ADP) and ionized impurity (IMP) scattering, the differential scattering rate is described by

τnk→mk+q−1=2πℏ∣gnm(k,q)∣2δ(εnk−εmk+q)(4)\tau^{-1}_{n\mathbf{k}\to m\mathbf{k}+\mathbf{q}} = \frac{2\pi}{\hbar} \lvert g_{nm}(\mathbf{k},\mathbf{q}) \rvert^2 \delta\left(\varepsilon_{n\mathbf{k}}-\varepsilon_{m\mathbf{k}+\mathbf{q}}\right) \tag*{(4)}

In this case, the delta function ensures energy conservation without phonon exchange.

The electron-phonon coupling matrix element gnm(k,q)g_{nm}(\mathbf{k},\mathbf{q}) was computed using a densely interpolated grid of 95×95×4995 \times95 \times49 kk-points, combined with material parameters obtained from first-principles calculations. This matrix element incorporates contributions from three primary scattering mechanisms: ADP, POP, and IMP.

gADP(k,q)=[kBTεd2B]12⟨ψnk∣ψmk+q⟩(5)g^{ADP}(\mathbf{k},\mathbf{q}) = \left[\frac{k_{\mathrm{B}}T\varepsilon_d^2}{B}\right]^{\frac{1}{2}}\langle\psi_{n\mathbf{k}} \mid\psi_{m\mathbf{k}+\mathbf{q}}\rangle \tag*{(5)}
gIMP(k,q)=[e2niiεs2∣⟨ψnk∣ψmk+q⟩∣2∣q∣2+β2](6)g^{IMP}(k,q)=\left[\frac{e^{2}n_{ii}}{\varepsilon_{s}^{2}}\frac{\left|\langle\psi_{nk}|\psi_{mk+q}\rangle\right|^{2}}{|q|^{2}+\beta^{2}}\right] \tag*{(6)}
gPOP(k,q)=[ℏωpo2(1ε∞−1εs)]∣⟨ψnk∣ψmk+q⟩∣∣q∣(7)g^{POP}(k,q)=\left[\frac{\hbar\omega_{po}}{2}\left(\frac{1}{\varepsilon_{\infty}}-\frac{1}{\varepsilon_{s}}\right)\right]\frac{\left|\langle\psi_{nk}|\psi_{mk+q}\rangle\right|}{|q|} \tag*{(7)}

where kBk_{B}, εd\varepsilon_{d}, BB, niin_{ii}, β\beta, ωpo\omega_{po}, ε∞\varepsilon_{\infty} and εs\varepsilon_{s} represent the Boltzmann constant, deformation potential, bulk modulus, concentration of ionized impurities, inverse screening length, optical phonon frequency, high-frequency dielectric constant, and static dielectric constant, respectively. ⟨ψnk∣ψmk+q⟩\langle\psi_{nk}|\psi_{mk+q}\rangle denotes the overlap integral between the initial and final electronic wavefunctions ψnk\psi_{nk} and ψmk+q\psi_{mk+q}, which reflects the transition probability between electronic states due to electron-phonon interactions.

Resluts and discussion

Crystal Configuration and Lattice Distortion

AgXTe2_2 (X=In, Ga) is a tetragonal crystal with a space group of I4ˉ2dI\bar{4}2d. As illustrated in Figure 1(a), the chalcopyrite structure of AI^{I}BIII^{III}X2VI_2^{VI} is derived from the binary cubic zincblende structure of ZnSe (F4ˉ3d\bar{4}3d). This transformation occurs through the substitution of two Zn atoms with elements from group I (e.g. Cu or Ag) and group III (e.g. Ga, or In). Subsequently, two substituted zincblende unit cells are stacked and extended along the c-direction, resulting in the formation of a tetragonal chalcopyrite structure [43, 44]. For AgXTe2_2, it features three distinct types of characteristic tetrahedra: [TeAg2_2X2_2]6+^{6+}, [XTe4_4]5−^{5-}, and [AgTe4_4]7−^{7-}. These tetrahedra are arranged in a specific manner within the chalcopyrite lattice. The [XTe4_4]5−^{5-} and [AgTe4_4]7−^{7-} tetrahedra are linked together to form a 3D framework by sharing corners of the Te atoms [45, 46]. This structure typically exhibits strong anharmonicity due to the distortion of tetrahedra formed by the linkage of different atoms [28].

Schematic representation of the chalcopyrite crystal structure and pressure dependence of the tetragonal distortion parameter

Figure 1. (a) Schematic representation of the chalcopyrite crystal structure. Adjacent to the structure are three smaller tetrahedra, representing the coordination environments of [TeAg2_2X2_2]6+^{6+}, [XTe4_4]5−^{5-}, and [AgTe4_4]7−^{7-}, respectively. These tetrahedral configurations illustrate the local bonding arrangements within the crystal structure. (b) Pressure dependence of the tetragonal distortion parameter η\eta for the chalcopyrite compounds AgInTe2_2 and AgGaTe2_2. The inset illustrates the pressure-induced distortion of the [TeAg2_2X2_2]6+^{6+} tetrahedral unit in AgXTe2_2.

Previous investigations have demonstrated that AgInTe2_2 and AgGaTe2_2 maintain structural stability within the pressure ranges of 0-4 GPa and 0-3.8 GPa, respectively [47]. Herein, we choose the corresponding phase-transition pressure points to investigate the influence of hydrostatic pressure on the properties of AgInTe2_2 and AgGaTe2_2. First, we observed that both lattice parameters and bond lengths exhibit varying degrees of reduction under the influence of pressure, as shown in Table I. (The trend of the lattice constant and volume as a function of pressure is shown in Fig. S1 [48]). Interestingly, the tetrahedral units observed deviate from ideal ortho-tetrahedral geometry, exhibiting slight distortions, as illustrated in Fig. S2. Generally, the distortions of tetrahedral units are linked to the so-called lattice distortion parameter η=∣2−c/a∣\eta=|2-c/a|, which as an indicator of the deviation degree, as shown in Figure 1(b). This structural distortion arises from the weak hybridization of sd3sd^{3} orbitals of the Ag atom, causing the atoms to deviate from the tetrahedral center [28]. Consequently, this deviation contributes to the overall distortion of the crystal, leading to strong acoustic and optical phonon scattering. The results demonstrate that the AgGaTe2_2 system exhibits higher sensitivity to pressure with lattice distortion parameter gradually increases with increasing pressure, indicating that the structure is distorted more under pressure. On the contrary, the lattice distortion parameter of AgInTe2_2 remains relatively constant under pressure. While structural distortions typically lead to increased phonon scattering, we anticipate a significant reduction in lattice thermal transport under pressure, particularly in the case of AgGaTe2_2.

Lattice Thermal Conductivity

To investigate this correlation, we calculated the lattice thermal conductivity of AgXTe2_2 (X=In, Ga) under pressure, as illustrated in Figure 2. The results indicate that the lattice thermal conductivity of AgInTe2_2 exhibits a monotonically decreasing trend under increasing pressure. Specifically, the κL\kappa_{L} decreases from 2.42 W/mK at 0 GPa to 1.02 W/mK at 4 GPa. This behavior suggests a continuous reduction in the ability of the lattice to conduct heat as pressure increases, due to enhanced phonon scattering or modifications in the phonon dispersion relations. In contrast, AgGaTe2_2 shows a non-monotonous trend in its κL\kappa_{L} under pressure. Initially, the κL\kappa_{L} increases from 2.08 W/mK at 0 GPa to 2.14 W/mK at 1 GPa, indicating that at lower pressures, there might be a stiffening of the lattice or reduced phonon scattering. However, beyond this point, the thermal conductivity decreases, reaching 1.49 W/mK at 3.8 GPa. This non-linear behavior suggests a more complex interaction between pressure and phonon dynamics, where an initial enhancement in thermal conductivity is followed by a reduction, possibly due to increased anharmonicity or changes in the structural properties at higher pressures. The insert figure illustrates the calculated κL\kappa_{\mathrm{L}} of AgXTe2_2 as a function of temperature under different pressures. It can be observed that in the temperature range of 300–800 K, the κL\kappa_{\mathrm{L}} decreases monotonically with increasing temperature. Additionally, we calculated the temperature dependence of the thermal conductivity under different pressures, and the predicted κL\kappa_{\mathrm{L}} follows a T−1T^{-1} temperature dependence.

Evolution of lattice thermal conductivity as a function of applied pressure for AgInTe2 and AgGaTe2 compounds at 300 K

Figure 2. The evolution of lattice thermal conductivity as a function of applied pressure for AgInTe2 and AgGaTe2 compounds at 300 K. And the two vertical lines represent the critical phase transition pressures for AgInTe2 and AgGaTe2, respectively. The insert illustrates the temperature-dependent behavior of lattice thermal conductivity for the material under two distinct pressure regimes: ambient pressure and the critical pressure associated with structural phase transition.

Subsequently, we investigated the phonon dispersion curves at different pressures to explain the change, as illustrated in Figure 3 and Fig. S3. At ambient pressure, AgXTe2_2 (X=In, Ga) exhibits flat modes in their low-frequency regions of their phonon dispersion, involving both low-lying optical phonons and acoustic phonons [49, 50]. This flatness suggests an increased number of phonon modes capable of participating in scattering processes while fulfilling energy and momentum conservation laws, thereby maximizing the phonon-phonon scattering channels [51]. Notably, the application of pressure induces softening of low-energy phonons and broadens their bandwidth (highlighted by the shaded region in the figure), which encompasses the acoustic phonons and the twelve lowest-lying optical branches.

Phonon dispersion curves of AgInTe2 and AgGaTe2 at different pressures

Figure 3. Phonon dispersion curves of (a) AgInTe2_2 at 0 GPa, (b) AgInTe2_2 at 4 GPa, (c) AgGaTe2_2 at 0 GPa, and (d) AgGaTe2_2 at 3.8 GPa. The color scale represents the projection of the phonon group velocity for each mode, with maximum group velocities of 3.42 km/s for AgInTe2_2 and AgGaTe2_2.

For AgInTe2_2, this bandwidth expands from 30.1 cm−1^{-1} to 36 cm−1^{-1} under pressure. In contrast, the bandwidth expansion in AgGaTe2_2 is more moderate, increasing from 41.1 cm−1^{-1} to 42.8 cm−1^{-1}. The manifestation of this change will be demonstrated later, as we currently focus on a simplified phonon relations. Assuming the phonon group velocity is given by the derivative of the phonon frequency concerning the wave vector qq, flat bands correspond to regions of low group velocity across the phonon branches in both AgInTe2_2 and AgGaTe2_2. Based on the color mapping of the projected phonon modes, the phonon group velocities in AgInTe2_2 are slightly lower than those in AgGaTe2_2 in the low-frequency range below 50 cm−1^{-1}. Upon the application of pressure, both materials exhibit significant softening of their acoustic phonons, accompanied by a modest reduction in group velocity.

In the high-frequency region (above 120 cm−1^{-1}), both materials exhibit a pronounced optical phonon frequency gap, which is attributed to the atomic mass difference between AgInTe2_2 and AgGaTe2_2. Upon applying pressures of 4 GPa and 3.8 GPa, both materials exhibit hardening of the high-frequency optical branches. However, the optical phonon frequency gap in AgInTe2_2 decreases under pressure, whereas it widens in AgGaTe2_2. This contrasting behavior arises from the faster hardening rate of the high-frequency optical branches compared to the mid-frequency optical branches. In the mid-frequency range (50–120 cm−1^{-1}), we observed a significant hardening of the phonon branches under applied pressure, accompanied by a significant increase in group velocity. This phenomenon arises from the combined influence of the softening of optical branches in the low-frequency regime and the hardening of optical branches in the high-frequency regime, which together account for the substantial increase in group velocity in the mid-frequency region.

The lattice thermal conductivity spectra and cumulative thermal conductivity of AgXTe2_2 under pressure were calculated, as shown in Figure 4(a-Figure 4b). At ambient pressure, AgInTe2_2 exhibited a higher κL\kappa_{\mathrm{L}} of 2.41 W/mK compared to 2.05 W/mK for AgGaTe2_2. This difference can be attributed to variations in their phonon spectra in the low-frequency region [52, 53]. As illustrated in Figure 4(a), the κL\kappa_{\mathrm{L}} of AgInTe2_2 is predominantly determined by phonons in the frequency range of 0-30 cm−1^{-1}. When subjected to pressure, a notable alteration in the thermal conductivity spectrum is observed. At 4 GPa, the frequency range contributing to κL\kappa_{\mathrm{L}} expands to 0-50 cm−1^{-1}. This expansion indicates an increase in the phonon scattering rate and available phase space within this extended range. Such findings are consistent with the observed softening and broadening of low-energy phonons in the phonon spectra. In contrast, as illustrated in Figure 4(b), the thermal conductivity spectrum of AgGaTe2_2 at 3.8 GPa showed relatively minor changes in the low-frequency region. We observed a slight enhancement in the thermal conductivity contribution within the mid-frequency range (80-120 cm−1^{-1}). This observation can be attributed to the augmented phonon group velocity in the corresponding mid-frequency region of the phonon dispersion curves (Figure 3), which aligns with previous analyses. And the AgInTe2_2 is same observation applies as well. Furthermore, additional analysis indicates that the pressure dependence of κL\kappa_{\mathrm{L}} in the two materials exhibits significant discrepancies. AgInTe2_2 exhibits a more pronounced decrease in κL\kappa_{\mathrm{L}} under pressure, dropping by 57% at 4 GPa, while the κL\kappa_{\mathrm{L}} of AgGaTe2_2 decreases more moderately, by 28% at 3.8 GPa. This disparity can be attributed to variations in phonon scattering rates and phase space under pressure for the two materials.

Phonon properties of AgInTe$_2$ and AgGaTe$_2$ under ambient and high pressure conditions

Figure 4. Phonon properties of AgInTe2_2 and AgGaTe2_2 were investigated under ambient and high pressure conditions.(a, b) Lattice thermal conductivity spectra and cumulative lattice thermal conductivity with respect to frequency for AgInTe2_2 and AgGaTe2_2, revealing the contributions of different phonon modes to heat conduction. The blue line represents 0 GPa, while the yellow line represents the phase transition pressure for each respective material. (c, d) The three-phonon scattering rates for AgInTe2_2 and AgGaTe2_2 at 300 K under varying pressures are depicted, with the purple points representing 0 GPa and the blue points corresponding to their respective phase transition pressures. The black dashed line reflects the assumption that the phonon mode scattering rates are twice their frequencies, as predicted by the Cahill-Watson-Pohl model, commonly referred to as the Cahill limit or the amorphous limit.(e, f) Energy- and momentum-conserving three-phonon scattering phase space at 300 K under varying pressure, with the purple points representing 0 GPa and the blue points corresponding to their respective phase transition pressures. The insert figure illustrates the ratio of three-phonon phase space under 4 GPa and 0 GPa conditions, focusing on the low-frequency range.

To elucidate the observed discrepancies, the three-phonon scattering rates and scattering phase spaces were calculated for both materials under varying pressure conditions, as illustrated in Figure 4(c-Figure 4f). Figure 4(c-Figure 4d) clearly demonstrate that upon compression, both materials exhibit an increased phonon scattering rate at the crossover. between the acoustic and optical branches, albeit to differing degrees. This increase would contribute to the reduction in lattice thermal conductivity. Notably, this frequency range lies at the boundary between acoustic and low-frequency optical phonons, suggesting that the coupling between acoustic and low-frequency optical phonons is enhanced under pressure. The prominent contribution of Ag and Te atomic phonon density of states at the acoustic-optical phonon crossover in the phonon dispersion curves substantiates that Ag and Te atom-induced low-lying optical phonon branches are responsible for the strong coupling between acoustic and optical phonons, as shown in Figure 3. The coupling of these modes contributes to an expanded scattering phase space and leads to additional scattering events. [54] The changes in phase space indicate that modes with larger phase space facilitate a greater number of scattering events, resulting in higher scattering rates. At a pressure of 4 GPa, AgInTe2_2 exhibits a significant expansion of its scattering phase space within the low-frequency region of 0–75 cm−1^{-1}, as shown in Figure 4(e). This expansion reflects a substantial increase in the number of three-phonon interaction channels satisfying energy and momentum conservation within this frequency range, a prerequisite for enhanced three-phonon scattering processes. While AgGaTe2_2 also exhibits a moderate increase in scattering phase space at a pressure of 3.8 GPa, the magnitude of this change is considerably smaller compared to that observed in AgInTe2_2.

Pressure-induced Metavalent Bonding and Anharmonicity

The degree of lattice distortion within a crystal structure plays a significant role in phonon transport. Generally, a higher degree of lattice distortion corresponds to lower κL\kappa_L. This relationship can be summarized as: increased structural complexity leads to reduced κL\kappa_L. Under ambient pressure conditions, both AgGaTe2_2 and AgInTe2_2 appear to follow this trend, with the more distorted AgGaTe2_2 exhibiting lower κL\kappa_L. However, this correlation does not hold true under high pressure. Despite exhibiting a larger lattice distortion parameter than AgInTe2_2 at high pressure, AgGaTe2_2 surprisingly demonstrates higher κL\kappa_L. This deviation suggests that under high-pressure conditions, factors beyond lattice distortion, such as changes in phonon scattering mechanisms or electronic contributions to thermal conductivity, may become more dominant in influencing κL\kappa_L.

To explore the underlying mechanisms responsible for the observed significant discrepancies in the lattice thermal conductivity of AgInTe2_2 and AgGaTe2_2 under pressure, a comparative analysis of their transport properties under pressure was conducted, as illustrated in Figure 5. As shown in Figure 5(a), the three-phonon scattering rates of

Three-panel comparison of phonon scattering properties for AgInTe₂ and AgGaTe₂

Figure 5. A comparative analysis of the phonon scattering properties of AgInTe2_2 (red circles) and AgGaTe2_2 (blue circles) at their respective phase transition pressures. (a) Three-phonon scattering rates; the orange dashed line reflects the assumption that the phonon mode scattering rates are twice their frequencies, commonly referred to as the Cahill limit. (b) Grüneisen parameters. (c) Available phase space for three-phonon scattering processes. These properties provide insights into the anharmonic lattice dynamics of each material.

AgInTe2_2 and AgGaTe2_2 at room temperature of 4 GPa and 3.8 GPa, respectively. We find that the scattering rate of AgInTe2_2 is much larger than that of AgGaTe2_2 in the low-frequency region, which explains why the change in thermal conductivity of AgInTe2_2 is more sensitive at high pressures. In order to explore which parameter has a greater effect on the scattering rate, we discuss below the effect of the three-phonon scattering phase space and the Grüneisen parameter on the scattering rate. The Grüneisen parameter, γλ\gamma_\lambda, is expressed as:

γλ=−16ωλ2∑k∑l′k′∑l′′k′′∑αβγ[Φαβγ(0k,l′k′,l′′k′′)eαkλeβk′λ′MkMk′eiqRl′rl′′k′′γ](8)\gamma_\lambda=-\frac{1}{6\omega_\lambda^2}\sum_k\sum_{l'k'}\sum_{l''k''}\sum_{\alpha\beta\gamma}\left[\Phi_{\alpha\beta\gamma}(0k,l'k',l''k'')\frac{e_{\alpha k}^{\lambda}e_{\beta k'}^{\lambda'}}{\sqrt{M_kM_{k'}}}e^{iqR_{l'}}r_{l''k''}^{\gamma}\right] \tag*{(8)}

where Φαβγ(0k,l′k′,l′′k′′)\Phi_{\alpha\beta\gamma}(0k,l'k',l''k'') is third-order interatomic force constant (IFC) tensor, eαkλe_{\alpha k}^{\lambda} is polarization vector of the phonon mode λ\lambda at atomic site kk in the α\alpha direction, eβk′λ′e_{\beta k'}^{\lambda'} is polarization vector of another phonon mode λ′\lambda' at atomic site k′k' in the β\beta direction, eiqRl′e^{iqR_{l'}} is a phase factor related to the position of the atom at site l′l', rl′′k′′γr_{l''k''}^{\gamma} is displacement vector of the atom at site l′′l'' in the γ\gamma direction. It is worth noting that the Grüneisen parameter of AgInTe2_2 is very much larger than that of AgGaTe2_2, about more than three times that of AgGaTe2_2, which implies a greater anharmonicity of AgInTe2_2.

The phase space (Wλ±W_\lambda^{\pm}) for three-phonon scattering is defined as the sum of the frequency factors associated with the expression (Γλλ′λ′′±\Gamma_{\lambda\lambda'\lambda''}^{\pm}), given by:

Wλ±=12N∑λ′λ′′{2(fλ′−fλ′′)fλ′+fλ′′+1}×δ(ωλ±ωλ′−ωλ′′)ωλωλ′ωλ′′(9)W_\lambda^{\pm}=\frac{1}{2N}\sum_{\lambda'\lambda''}\left\{\frac{2(f_{\lambda'}-f_{\lambda''})}{f_{\lambda'}+f_{\lambda''}+1}\right\}\times\frac{\delta(\omega_\lambda\pm\omega_{\lambda'}-\omega_{\lambda''})}{\omega_\lambda\omega_{\lambda'}\omega_{\lambda''}} \tag*{(9)}

Where fλ′f_{\lambda'} and fλ′′f_{\lambda''} are Fermi-Dirac distribution functions, δ(ωλ±ωλ′−ωλ′′)\delta(\omega_\lambda\pm\omega_{\lambda'}-\omega_{\lambda''}) is the Dirac delta function, the denominator ωλωλ′ωλ′′\omega_\lambda\omega_{\lambda'}\omega_{\lambda''} is the product of the frequencies, typically used for normalization or representing the reciprocal of energy units. The phonon scattering phase space at high pressure shows that the data obtained for AgInTe2_2, is much larger than that of AgGaTe2_2, indicating that the phonon dispersion curves of AgInTe2_2 at pressure better satisfy the energy conservation and momentum conservation.

To further investigate the bonding characteristics, we computed the shared and transform charge for both compounds, as depicted in Table II. Analysis indicates a stronger Ag-Te bond in AgInTe2_2 at ambient pressure than in AgGaTe2_2. Conversely, the Ga-Te bond exhibits a greater degree of charge sharing than the In-Te bond, suggesting a slightly stronger interaction in the former case. Notably, the In compound exhibits a larger charge transfer than the Ga compound, which can be attributed to the higher electronegativity of Ga. In addition, both compounds show an increasing trend in charge transfer with increasing pressure. Metavalent bonding, distinct from covalent or metallic bonding, characterizes these compounds. A defining feature of metavalent bonds is their high degree of anharmonicity, which exhibits a positive correlation with the extent of charge transfer within the compound. The deviation from an ideal tetrahedral structure underpins the formation of metavalent bonds. Consequently, AgInTe2_2 exhibits stronger anharmonicity than AgGaTe2_2 under both ambient and high-pressure conditions. However, it is noteworthy that despite its weaker anharmonicity, AgGaTe2_2 displays lower lattice thermal conductivity than AgInTe2_2 under ambient pressure. This phenomenon can be attributed to the more complex structural characteristics of AgGaTe2_2 under standard conditions.

Pressure (GPa)Transferred charge (∣e∣|e|)Shared charges (∣e∣|e|)
AgIn or GaTeAg-TeIn/Ga-Te
AgInTe2_200.1910.542-0.3670.9140.970
40.1960.552-0.3741.0181.041
AgGaTe2_200.1650.420-0.2930.9100.992
3.80.1720.426-0.2990.9951.053

Table II. The transferred charge and shared charges (∣e∣|e|) of AgInTe2_2 and AgGaTe2_2 at 0 and 4 (3.8) GPa calculated using chargmol.

Electrical Transport and Electron-phonon Scattering

Next we explore the effect of pressure on the electronic structure of AgInTe2_2 and AgGaTe2_2. Figure 6(a-Figure 6b) displays the electronic band structure and the density of states under hydrostatic pressure. The computed bandgap values at atmospheric pressure are 0.87 eV for AgInTe2_2 and 1.03 eV for AgGaTe2_2, respectively. Due to the quantum size effect [55], the application of pressure causes a slight increase in the band gap, which increases to 1.05 eV and 1.3 eV at 4 GPa and 3.8 GPa, respectively. Analogous behavior is exhibited in other chalcopyrite materials, such as CuInTe2_2, where the band gap undergoes a notable expansion from 1.03 eV to 1.44 eV under an applied pressure of 7.6 GPa [30]. The pressure coefficient of the bandgap, denoted as ΔEg/ΔP\Delta E_g/\Delta P, quantifies the responsiveness of the bandgap to variations in applied pressure. For AgInTe2_2 and AgGaTe2_2, the respective pressure coefficients for bandgap widening are 45 meV/GPa and 71 meV/GPa. The notably higher value for AgGaTe2_2 suggests a greater sensitivity of its bandgap to pressure-induced changes compared to AgInTe2_2. This difference in pressure sensitivity may arise from variations in the compressibility and bonding characteristics between the two materials, leading to distinct responses to applied pressure in terms of their electronic properties. In addition, the valence band becomes more dispersive under pressure, which will greatly improve the increase in σ\sigma. In addition, from the density of states in the electronic band structures, it is evident that the valence band maximum in both AgInTe2_2 and AgGaTe2_2 is primarily contributed by Te and Ag atoms, with a negligible contribution from In atoms. This contribution remains largely unchanged under the influence of applied pressure.

Pressure-dependent electronic structure and carrier mobility in AgInTe2 and AgGaTe2

Figure 6. Pressure-Dependent Electronic Structure and Carrier Mobility in AgInTe2_2 and AgGaTe2_2. (a)-(b) Calculated band structures and densities of states at atmospheric pressure (dashed lines) and the phase transition pressure (solid lines). (c)-(d) Calculated carrier mobility, including contributions from different scattering mechanisms and the total mobility, at 0 GPa (dashed lines) and the phase transition pressure (solid lines).

Furthermore, pressure not only preserves but also improves the electronic transport properties. To illustrate this phenomenon, the hole mobility was calculated by incorporating ADP, POP, and IMP scattering mechanisms to accurately model electrical transport characteristics. Figure 6(c-Figure 6d) illustrates the total and partial hole mobilities limited by the respective scattering mechanisms. In AgInTe2_2, the magnitudes of the three scattering mechanisms are comparable, resulting in a significant influence on the total hole mobility, as illustrated in Figure 6(c). Under pressure, ADP scattering increases substantially, followed by enhancements in IMP and POP scattering, resulting in a marked improvement in total hole mobility. For AgGaTe2_2, although the improvement in IMP scattering due to pressure is minimal, the substantial enhancements in ADP and POP significantly contribute to the overall increase in hole mobility. The significant enhancement in hole mobility is attributed to the combined effect of reduced single-band effective mass and deformation potential constant, stemming from pressure-induced tetrahedral distortion [56]. In the chalcopyrite systems under investigation, POP scattering emerges as the dominant mechanism controlling hole mobility, consistent with recent reports on polar systems such as PbTe [57], SnSe [58], ReCuZnP2_2 [59], and several half-and full-Heusler compounds [60]. Additionally, we calculated κe\kappa_{\mathrm{e}}, SS, κL\kappa_{\mathrm{L}}, and PFPF, as presented in Fig. S4 of the supplementary material.

Power Factor and Figures of Merit

Subsequently, we conducted an extensive analysis of the pressure-dependent PFPF performance to elucidate this relationship quantitatively. Figure 7(a-Figure 7b) showcase heat maps that vividly illustrate the intricate variations in carrier concentration and power factor change (ΔPF=PFP−PF0\Delta PF = PF_P - PF_0) as a function of applied pressure at 900 K. Our findings reveal a striking contrast between AgInTe2_2 and AgGaTe2_2. The former exhibits a remarkably larger PFPF enhancement, with a maximum increase of approximately 2.1 mW m−1^{-1} K−2^{-2} at a carrier concentration of 6.21 ×\times 1020^{20} cm−3^{-3}. This substantial improvement underscores the potential of AgInTe2_2 as a highly responsive material to pressure-induced optimization. Conversely, AgGaTe2_2, while demonstrating a more modest enhancement, still achieves a noteworthy optimal increase of about 1 mW m−1^{-1} K−2^{-2} at 7.88 ×\times 1020^{20} cm−3^{-3} and 3.8 GPa.

Calculated changes in power factor and thermoelectric figure of merit for AgInTe2 and AgGaTe2

Figure 7. The calculated ΔPF\Delta PF of (a) AgInTe2_2 and (b) AgGaTe2_2 as a function of carrier concentration and pressure at 900 K. The ΔZT\Delta ZT of (c) AgInTe2_2 and (d) AgGaTe2_2 as a function of carrier concentration and pressure at 900 K. Where ΔPF=PFP−PF0\Delta PF = PF_P - PF_0, ΔZT=ZTP−ZT0\Delta ZT = ZT_P - ZT_0, the change in color in the graph indicates the magnitude of the ΔPF\Delta PF and ΔZT\Delta ZT changes.

Intriguingly, both compounds exhibit maximum optimization near their respective phase transition pressures and in heavily doped regions. This convergence of optimal conditions suggests a principle in pressure-tuned thermoelectrics: the synergistic effect of structural changes and high carrier concentrations can lead to significant performance enhancements. Such a finding opens new avenues for designing high-performance thermoelectric materials tailored for extreme conditions.

To provide a holistic view of the thermoelectric potential, we extended our analysis to the thermoelectric ZTZT, a crucial parameter for assessing overall thermoelectric efficiency. Figure 7(c-Figure 7d) present our predictions for ΔZT\Delta ZT (ΔZT=ZTP−ZT0\Delta ZT = ZT_P - ZT_0) at 900 K as a function of hole concentration, offering insights into the optimal doping levels under pressure. Furthermore, the dependence of the thermoelectric ZTZT of AgXTe2_2 on carrier concentration under various pressures was calculated, as illustrated in Supplementary Fig. S5. The results for AgInTe2_2 are particularly striking. We observe a remarkable ZTZT enhancement of 1.98 at a hole concentration of 2.21 ×\times 1019^{19} cm−3^{-3} and 900 K. Even more impressive is the peak ZTZT value of 3.31, achieved under an applied pressure of 4 GPa and a concentration of 3.56 ×\times 1019^{19} cm−3^{-3}. This surprising enhancement showcases the transformative potential of pressure tuning in thermoelectric materials. While the ZTZT enhancement in AgGaTe2_2 is less dramatic, it is not insignificant. The inherently excellent thermoelectric properties of the compound at ambient pressure offer a robust foundation. Coupled with pressure modulation, this results in a maximum ZTZT value of 2.44 at 900 K and a hole concentration of 4.52 ×\times 1019^{19} cm−3^{-3}. In Figure 8, we compare the ZTZT values of AgXTe2\mathrm{AgXTe}_{2} (X=InX=\mathrm{In}, Ga\mathrm{Ga}) with those of conventional thermoelectric materials [30, 61, 62, 63]. The data indicate that pressure-tuned AgInTe2\mathrm{AgInTe}_{2} achieves competitive ZTZT values, reinforcing its potential as a high-performance thermoelectric material. Our result underscores the importance of considering both intrinsic material properties and external tuning parameters in the quest for high-performance thermoelectrics. These findings not only clarify the pressure-dependent behavior of AgXTe2\mathrm{AgXTe}_{2} (X=InX=\mathrm{In}, Ga\mathrm{Ga}) compounds but also contribute to the broader understanding of structure-property relationships in thermoelectric materials.

Maximum ZT values of AgXTe2 (X=In, Ga) and comparison compounds under ambient and applied pressure

Figure 8. Maximum ZTZT values of AgXTe2_2 (X=In, Ga) [This work], CuInTe2_2 [30], CuFeS2_2 [61], CuGaTe2_2 [62], SnSe, Cu2_2Se, GeTe, and CoSb3_3 [63] under ambient and applied pressure. Ambient pressure results are indicated by the blue-green gradient, while pressure-tuned results are represented by the purple section.

Conclusions

In summary, the thermal transport and electrical transport properties of Ag-based chalcopyrite materials were studied using the first-principles calculation combined with the Boltzmann transport equation. The results reveal that AgInTe2\mathrm{AgInTe}_{2} exhibits superior lattice rigidity and consequently undergoes less lattice distortion under pressure compared to AgGaTe2\mathrm{AgGaTe}_{2}, which possesses weaker lattice rigidity. This phenomenon can be attributed to the stronger bonding strength of Ag-Te in the AgInTe2\mathrm{AgInTe}_{2} lattice compared to that in AgGaTe2\mathrm{AgGaTe}_{2}, resulting in a more resilient structure that is less susceptible to deformation under applied pressure. Moreover, the pressure-induced softening of low-frequency phonons significantly increases the low-frequency three-phonon scattering channels, greatly enhancing the coupling between acoustic and optical phonons, leading to a sharp decrease in lattice thermal conductivity. Interestingly, the positive correlation between lattice distortion and lattice thermal conductivity observed at ambient pressure does not appear to hold under high pressure. Despite maintaining structural symmetry under high pressure, AgInTe2\mathrm{AgInTe}_{2} exhibits lower lattice thermal conductivity than AgGaTe2\mathrm{AgGaTe}_{2}, which has a higher degree of lattice distortion, due to the enhanced anharmonicity induced by high pressure. Under the influence of hydrostatic pressure, the ZTZT values of AgInTe2\mathrm{AgInTe}_{2} and AgGaTe2\mathrm{AgGaTe}_{2} exhibited remarkable enhancements. Surprisingly, the maximum ZTZT value of AgInTe2\mathrm{AgInTe}_{2} increased by approximately 90% while that of AgGaTe2\mathrm{AgGaTe}_{2} improved by around 27%. These significant improvements in the thermoelectric performance under hydrostatic pressure conditions underscore the potential of pressure-induced optimization in chalcopyrite-type thermoelectric materials. The significant enhancements observed under pressure highlight the potential for developing next-generation thermoelectric devices capable of operating efficiently under extreme conditions, paving the way for novel applications in energy harvesting and thermal management.

Acknowledgments

The authors thank the National Natural Science Foundation of China (No. 52072188), the Program for Science and Technology Innovation Team in Zhejiang (No. 2021R01004), and acknowledge the institute of high-pressure physics of Ningbo University for its computational resources. sure, (2) The optimized crystal structures of AgXTe2AgXTe_{2} along the cc-axis, (3)Phonon dispersion curves under pressures of 1–3 GPa, (4) The Seebeck coefficient, electrical conductivity, and power factor as functions of pressure and doping concentration, (5) The calculated ZTZT values for AgXTe2AgXTe_{2}.

References

  1. [1]L. E. Bell, Cooling, heating, generating power, and recovering waste heat with thermoelectric systems, Science 321, 1457 (2008).DOI
  2. [2]D. M. Rowe, Thermoelectrics handbook: macro to nano (CRC Press, 2005).
  3. [3]J. Yue, J. Zheng, J. Li, S. Guo, W. Ren, H. Liu, Y. Liu, and T. Cui, Ultralow Glassy thermal conductivity and controllable, promising thermoelectric properties in crystalline o-CsCu5S3, ACS Appl. Mater. Interfaces 16, 20597 (2024).DOI
  4. [4]H. Azimi, Y. Hou, and C. J. Brabec, Towards low-cost, environmentally friendly printed chalcopryite and kesterite solar cells, Energy Environ. Sci. 7, 1829 (2014).DOI
  5. [5]G. J. Snyder and E. S. Toberer, Complex thermoelectric materials, Nat. Mater. 7, 105 (2008).DOI
  6. [6]A. Zhang, Y. Cui, J. Yue, J. Li, Y. Pan, X. Chen, Y. Liu, and T. Cui, Pressure-induced enhancement of thermoelectric performance of CoP3 by the structural phase transition, Acta Mater. 248, 118773 (2023).DOI
  7. [7]C. Chang and L.-D. Zhao, Anharmonicity and low thermal conductivity in thermoelectrics, Mater. Today Phys. 4, 50 (2018).
  8. [8]X. Shi, L. Chen, and C. Uher, Recent advances in high-performance bulk thermoelectric materials, Int. Mater. Rev. 61, 379 (2016).DOI
  9. [9]W. Gao, Z. Wang, J. Huang, and Z. Liu, Extraordinary thermoelectric performance realized in hierarchically structured AgSbSe2 with ultralow thermal conductivity, ACS Appl. Mater. Interfaces 10, 18685 (2018).DOI
  10. [10]J. Li, J. Yue, S. Guo, A. Zhang, L. Zhu, H. Song, Z. Liu, Y. Liu, and T. Cui, High-temperature superconductivity of boron-carbon clathrates at ambient pressure, Phys. Rev. B 109, 144509 (2024).DOI
  11. [11]C. Deng, M. Wang, H. Huang, M. Xu, W. Zhao, M. Du, H. Song, and T. Cui, High-Tc superconductors in the ternary Sr-Hf/Zr-H system at high pressure, Phys. Rev. B 109, 184516 (2024).DOI
  12. [12]Y. Zhou, Z.-Y. Dong, W.-P. Hsieh, A. F. Goncharov, and X.-J. Chen, Thermal conductivity of materials under pressure, Nat. Rev. Phys. 4, 319 (2022).DOI
  13. [13]W. Shi, T. Deng, G. Wu, K. H. Hippalgaonkar, J.-S. Wang, and S.-W. Yang, Unprecedented Enhancement of Thermoelectric Power Factor Induced by Pressure in Small-Molecule Organic Semiconductors, Adv. Mater. 31, 1901956 (2019).DOI
  14. [14]S. Li, Z. Qin, H. Wu, M. Li, M. Kunz, A. Alatas, A. Kavner, and Y. Hu, Anomalous thermal transport under high pressure in boron arsenide, Nature 612, 459 (2022).DOI
  15. [15]W. Cao, Z. Wang, L. Miao, J. Shi, and R. Xiong, Extremely anisotropic thermoelectric properties of SnSe under pressure, Energy Environ. Mater. 6, e12361 (2023).DOI
  16. [16]Y. Zhang, S. Hao, L.-D. Zhao, C. Wolverton, and Z. Zeng, Pressure induced thermoelectric enhancement in SnSe crystals, J. Mater. Chem. A 4, 12073 (2016).DOI
  17. [17]J. Ning, S. V. Kershaw, and A. L. Rogach, Synthesis and Optical Properties of Cubic Chalcopyrite/Hexagonal Wurtzite Core/Shell Copper Indium Sulfide Nanocrystals, J. Am. Chem. Soc. 141, 20516 (2019).DOI
  18. [18]H. Ferhati, F. Djefal, N. Boubiche, and F. Le Normand, An efficient ITO-free transparent electrode based on diamond-like carbon with an engineered intermediate metallic thin-film, Sol. Energy 196, 327 (2020).DOI
  19. [19]F. Stock, F. Antoni, D. Aubel, S. Hajjar-Garreau, and D. Muller, Pure carbon conductive transparent electrodes synthesized by a full laser deposition and annealing process, Appl. Surf. Sci. 505, 144505 (2020).DOI
  20. [20]S. Ishizuka and N. Taguchi, Aluminum-Based Chalcopyrite Thin Films and Solar Cells, Adv. Energy Mater. , 2400087 (2024).DOI
  21. [21]P. Qiu, Y. Qin, Q. Zhang, R. Li, J. Yang, Q. Song, Y. Tang, S. Bai, X. Shi, and L. Chen, Intrinsically high thermoelectric performance in AgInSe2 n-type diamond-like compounds, Adv. Sci. 5, 1700727 (2018).DOI
  22. [22]Y. Li, J. Liu, X. Wang, and J. Hong, Anomalous suppressed thermal conductivity in CuInTe2 under pressure, Appl. Phys. Lett. 119 (2021).DOI
  23. [23]T. Pildpring, K. Kurosaki, A. Kosuga, T. Day, S. Firdosy, V. Raj, G. J. Snyder, A. Harynunggmoung, T. Sugahara, Y. Ohishi, et al., Chalcopyrite CuGaTe2: a high-efficiency bulk thermoelectric material, Adv. Mater. 24, 3622 (2012).DOI
  24. [24]H. Xie, S. Hao, S. Cai, T. P. Bailey, C. Uher, C. Wolverton, V. P. Dravid, and M. G. Kanatzidis, Ultralow thermal conductivity in diamondoid lattices: high thermoelectric performance in chalcopyrite Cu0.8+yAg0.2In1−yTe2, Energy Environ. Sci. 13, 3693 (2020).
  25. [25]H. Xie, S. Hao, T. P. Bailey, S. Cai, Y. Zhang, T. J. Slade, G. J. Snyder, V. P. Dravid, C. Uher, C. Wolverton, et al., Ultralow thermal conductivity in diamondoid structures and high thermoelectric performance in (Cu1−xAgx)(In1−yGay)Te2, J. Am. Chem. Soc. 143, 5978 (2021).DOI
  26. [26]J. Zhang, L. Huang, C. Zhu, C. Zhou, B. Jabar, J. Li, X. Zhu, L. Wang, G. Song, H. Xin, et al., Design of domain structure and realization of ultralow thermal conductivity for record-high thermoelectric performance in chalcopyrite, Adv. Mater. 31, 1905210 (2019).DOI
  27. [27]L. Elalfy, D. Music, and M. Hu, Metavalent bonding induced abnormal phonon transport in diamondlike structures: Beyond conventional theory, Phys. Rev. B 103, 075203 (2021).DOI
  28. [28]H. Xie, E. S. Bozin, Z. Li, M. Abykoon, S. Banerjee, J. P. Male, G. J. Snyder, C. Wolverton, S. J. Billinge, and M. G. Kanatzidis, Hidden local symmetry breaking in silver diamondoid compounds is root cause of ultralow thermal conductivity, Adv. Mater. 34, 2202255 (2022).DOI
  29. [29]H. Yu, G. Huang, Q. Peng, L.-C. Chen, H.-J. Pang, X.-Y. Qin, P.-F. Qiu, X. Shi, L.-D. Chen, and X.-J. Chen, A combined experiment and first-principles study on lattice dynamics of thermoelectric CuInTe2, J. Alloys Compd. 822, 153610 (2020).DOI
  30. [30]J. Yue, S. Guo, J. Li, J. Zhao, C. Shen, H. Zhang, Y. Liu, and T. Cui, Pressure-induced remarkable four-phonon interaction and enhanced thermoelectric conversion efficiency in CuInTe2, Mater. Today Phys. 39, 101283 (2023).DOI
  31. [31]H. Yu, L.-C. Chen, H.-J. Pang, X.-Y. Qin, P.-F. Qiu, X. Shi, L.-D. Chen, and X.-J. Chen, Large enhancement of thermoelectric performance in CuInTe2 upon compression, Mater. Today Phys. 5, 1 (2018).DOI
  32. [32]G. Kresse and J. Furthmüller, Efficient iterative schemes for ab initio total-energy calculations using a plane-wave basis set, Phys. Rev. B 54, 11169 (1996).pubmed.ncbi.nlm.nih.gov/9984901
  33. [33]P. E. Blöchl, Projector augmented-wave method, Phys. Rev. B 50, 17953 (1994).pubmed.ncbi.nlm.nih.gov/9976227
  34. [34]P. Hohenberg and W. Kohn, Inhomogeneous electron gas, Phys. Rev. 136, B864 (1964).
  35. [35]J. P. Perdew, K. Burke, and Y. Wang, Generalized gradient approximation for the exchange-correlation hole of a many-electron system, Phys. Rev. B 54, 16533 (1996).pubmed.ncbi.nlm.nih.gov/9985776
  36. [36]J. P. Perdew, K. Burke, and M. Ernzerhof, Generalized gradient approximation made simple, Phys. Rev. Lett. 77, 3865 (1996).pubmed.ncbi.nlm.nih.gov/10062328
  37. [37]R. Pawar and A. A. Sangolkarr, Density functional theory based HSE06 calculations to probe the effects of defect on electronic properties of monolayer TMDCs, Comput. Theor. Chem. 1205, 113445 (2021).DOI
  38. [38]J. Yue, A. Zhang, J. Li, Y. Liu, and T. Cui, Significantly reinforced thermoelectric performance in the novel 1T-Au6Se2 monolayer, APL Mater. 11 (2023).DOI
  39. [39]A. Togo and I. Tanaka, First principles phonon calculations in materials science, Scr. Mater. 108, 1 (2015).arxiv.org/abs/1506.08498
  40. [40]W. Li, L. Lindsay, D. A. Broido, D. A. Stewart, and N. Mingo, Thermal conductivity of bulk and nanowire Mg2SixSn1−x alloys from first principles, Phys. Rev. B 86, 174307 (2012).DOI
  41. [41]W. Li, J. Carrete, N. Katcho, and N. Mingo, Sheng-BTE: A solver of the boltzmann transport equation for phonons, Comput. Phys. Commun. 185, 1747 (2014).
  42. [42]A. M. Ganose, J. Park, A. Faghaninia, R. Woodson, K. A. Persson, and A. Jain, Efficient calculation of carrier scattering rates from first principles, Nat. Commun. 12, 2222 (2021).DOI
  43. [43]J. Zhang, R. Liu, N. Cheng, Y. Zhang, J. Yang, C. Uher, X. Shi, L. Chen, and W. Zhang, High-performance pseudocubic thermoelectric materials from non-cubic chalcopyrite compounds, Adv. Mater. (2014).DOI
  44. [44]J. Jaffe and A. Zunger, Electronic structure of the ternary pnictide semiconductors ZnSiP2, ZnGeP2, ZnSnP2, ZnSiAs2, and MgSiP2, Phys. Rev. B 30, 741 (1984).
  45. [45]X. Su, N. Zhao, S. Hao, C. C. Stoumpos, M. Liu, H. Chen, H. Xie, Q. Zhang, C. Wolverton, X. Tang, et al., High thermoelectric performance in the wide band-gap AgGa1−xTex compounds: Directional negative thermal expansion and intrinsically low thermal conductivity, Adv. Funct. Mater. 29, 1806534 (2019).
  46. [46]H.-P. Liang, S. Geng, T. Jia, C.-N. Li, X. Xu, X. Zhang, and S.-H. Wei, Unveiling disparities and promises of Cu and Ag chalcopyrites for thermoelectrics, Phys. Rev. B 109, 035205 (2024).DOI
  47. [47]T. Bovornratanaraks, K. Kotmool, K. Yoodee, M. I. McMahon, and D. Ruffolo, High pressure structural studies of AgInTe2, J. Phys. Conf. Ser. 215, 012008 (2010).DOI
  48. [48]See Supplemental Material for more details on (1) variation of lattice constant and volume as functions of pres- sure, (2) The optimized crystal structures of AgXTe₂ along the c-axis, (3) Phonon dispersion curves under pressures of 1–3 GPa, (4) The Seebeck coefficient, electrical conductivity, and power factor as functions of pressure and doping concentration, (5) The calculated ZT values for AgXTe₂.
  49. [49]T. Tadano, Y. Gohda, and S. Tsuneyuki, Impact of rattlers on thermal conductivity of a thermoelectric clathrate: a first-principles study, Phys. Rev. Lett. 114, 095501 (2015).DOI
  50. [50]J. Feldman, D. Singh, I. Mazin, D. Mandrus, and B. Sales, Lattice dynamics and reduced thermal conductivity of filled skutterudites, Phys. Rev. B 61, R9209 (2000).DOI
  51. [51]W. Li and N. Mingo, Ultralow lattice thermal conductivity of the fully filled skutterudite YbFe₄Sb₁₂ due to the flat avoided-crossing filler modes, Phys. Rev. B 91, 144304 (2015).DOI
  52. [52]J. Yue, Y. Liu, W. Ren, S. Lin, C. Shen, H. K. Singh, T. Cui, T. Tadano, and H. Zhang, Role of atypical temperature-response lattice thermal transport on the thermoelectric properties of antiperovskites Mg₃XN (X=P, As, Sb, Bi), Mater. Today Phys. 41, 101340 (2024).DOI
  53. [53]J. Yue, J. Li, J. Zheng, X. Shen, W. Ren, G. H. Hautier, Y. Liu, and T. Cui, Hierarchical Characterization of Thermoelectric Performance in Copper-Based Chalcogenide CsCu₃S₂: Unveiling the role of Anharmonic Lattice Dynamics, Mater. Today Phys. 46, 101517 (2024).DOI
  54. [54]J. Yue, Y. Liu, and J. Zheng, High-order anharmonic scattering and wide-temperature-range glassy thermal transport in crystalline CsCu₄Se₃, arXiv preprint arXiv:2409.09594 (2024).
  55. [55]A. I. Efimov, A. L. Efros, and A. A. Onushchenko, Quantum size effect in semiconductor microcrystals, Solid State Commun. 56, 921 (1985).
  56. [56]J. Cao, J. D. Querales-Flores, A. R. Murphy, S. Fahy, and I. Savić, Dominant electron-phonon scattering mechanisms in n-type PbTe from first principles, Phys. Rev. B 98, 205202 (2018).DOI
  57. [57]J. Zhou, H. Zhu, T.-H. Liu, Q. Song, R. He, J. Mao, Z. Liu, W. Ren, B. Liao, D. J. Singh, et al., Large thermoelectric power factor from crystal symmetry-protected non-bonding orbital in half-Heuslers, Nat. Commun. 9, 1721 (2018).DOI
  58. [58]J. Ma, Y. Chen, and W. Li, Intrinsic phonon-limited charge carrier mobilities in thermoelectric SnSe, Phys. Rev. B 97, 205207 (2018).
  59. [59]J.-H. Pöhls, S. Chanakian, J. Park, A. M. Ganose, A. Dunn, N. Friesen, A. Bhattacharya, M. Hogan, S. Bux, A. Jain, et al., Experimental validation of high thermoelectric performance in ReCuZnP₂ predicted by high-throughput DFT calculations, Mater. Horiz. 8, 209 (2021).DOI
  60. [60]S. Guo, J. Yue, J. Li, Y. Liu, and T. Cui, Novel room-temperature full-Heusler thermoelectric material Li₂TiSb, Phys. Chem. Chem. Phys. 26, 6774 (2024).DOI
  61. [61]R. Li, X. Li, L. Xi, J. Yang, D. J. Singh, and W. Zhang, High-throughput screening for advanced thermoelectric materials: diamond-like ABX₂ compounds, ACS Appl. Mater. Interfaces 11, 24859 (2019).DOI
  62. [62]C. Chen, P. Zhang, L. Yue, J. Li, T. Fang, S. Zheng, and G. Lu, Computational prediction of high thermoelectric performance in p-type CuGaTe₂ with a first-principles study, Comput. Mater. Sci. 158, 369 (2019).DOI
  63. [63]Q. Tang, B. Jiang, K. Wang, W. Wang, B. Jia, T. Ding, Z. Huang, Y. Lin, and J. He, High-entropy thermoelectric materials, Joule (2024).DOI

Paper details

vlnc:W_b772e7rk
Version
v1 · latest
Published
Fresh — added to the Hub within the last 30 days
Added
License
CC BY 4.0
Usage

views · 0

downloads · 0

A view counts once per browser per day, a download each time the PDF is requested.

  • Physics and Astronomy

Not recorded for this paper

View statement
Looking for related papers…
Contents