Molecular beam epitaxy synthesis of ternary nitride PrTaN2_2 and its crystal structure determination

Abstract

We report the discovery of a novel ternary nitride PrTaN2_2 synthesized as a thin film using molecular beam epitaxy. The combination of e-beam evaporation for refractory elements and a radio-frequency nitrogen radical source enables growth under a highly nitriding environment, providing access to phases not readily obtained in bulk synthesis. Structural characterization by X-ray diffraction and high-angle annular dark-field scanning transmission electron microscopy reveals that the compound crystallizes in an orthorhombic structure and grows with a well-defined orientation on YAlO3_3 substrates, while remaining essentially strain-free. To determine the crystal structure from limited thin-film diffraction data, we developed a fitting procedure based on structure factors. By combining extinction rules with constraints from Wyckoff positions, the number of fitting parameters is significantly reduced, enabling reliable structure determination. Systematic exclusion of alternative candidate phases in the Pr-Ta-N system, together with structure factor fitting, identifies the space group as P222P222 and determines the atomic coordinates. The present results demonstrate that thin-film growth with molecular beam epitaxy can stabilize previously unexplored ternary nitrides, and establish a practical approach for structural determination in such systems. This work provides a pathway for the exploration of new complex nitride materials.

Introduction

Ternary complex nitrides with lanthanides are emerging and attracting attention as materials with rich physical properties.[1, 2, 3] The complex nitrides composed of lanthanides and group V–VII 5d5d transition metals (Ta, W, and Re) exhibit perovskite and Ruddlesden–Popper crystal structures.[4, 5, 6, 7, 8, 9] Analogous to oxide perovskite and Ruddlesden–Popper phases, these ternary nitrides are expected to show superconductivity, ferromagnetism, and ferroelectricity. However, despite many theoretical predictions of stable ternary nitrides,[10, 11, 12] the number of experimentally realized compounds remains limited. One major challenge is controlling group V–VII 5d5d transition metals during synthesis. The melting points of these elements exceed 3000 ∘C3000\,^{\circ}\mathrm{C}, making them difficult to handle. Another challenge is achieving sufficiently strong and pure nitridation conditions. For previously reported ternary nitrides, high pressure (∼8 GPa\sim8\,\mathrm{GPa}) and/or strong nitriding agents such as NaN3\mathrm{NaN}_{3} are required.[4, 5, 6, 7, 8, 9]

Here, we report the discovery of a novel ternary nitride PrTaN2\mathrm{PrTaN}_{2} achieved by thin film growth using molecular beam epitaxy (MBE). Compounds composed of lanthanides and tantalum have already been investigated in bulk form. [4, 5, 8] However, this particular phase has not been reported to date. This suggests that thin film growth provides access to phases that are not readily obtained in bulk synthesis. Our MBE system offers several advantages in addressing the challenges mentioned above. E-beam evaporators are available in our chamber, which can handle high-melting-point elements. Furthermore, a radical source using pure N2\mathrm{N}_2 provides favorable nitridation conditions. Compared with bulk growth using ammonia or azide, the effective nitrogen chemical potential can be higher in MBE because nitrogen is supplied in the form of reactive radical species. This provides a highly nitriding environment for film growth. These advantages enabled the discovery of the novel ternary nitride PrTaN2\mathrm{PrTaN}_2.

To confirm that the observed crystalline phase corresponds to a new material, we performed detailed X-ray diffraction (XRD) measurements and scanning transmission electron microscopy (STEM). There are multiple candidate phases in the Pr-Ta-N system other than PrTaN2\mathrm{PrTaN}_2. Detailed crystallographic analysis allows us to rule out these possible candidates. Furthermore, we determined the space group and atomic coordinates by developing a fitting procedure based on the structure factor. These findings open a new avenue for the exploration of novel ternary nitrides using thin film growth.

Methods

PrTaN2\mathrm{PrTaN}_2 thin films were grown on YAlO3\mathrm{YAlO}_3 (YAO) (001)c_\mathrm{c} substrates. For clarity in describing the substrate azimuth, we use the pseudo-cubic Miller index notation with the subscript "c". Our custom-designed MBE system is equipped with e-beam evaporators for generating Pr and Ta fluxes. Controlling the flux using e-beam evaporators is challenging due to the high melting point of tantalum (3017 °C). Nevertheless, the flux was precisely controlled using electron impact emission spectroscopy (EIES). [13] The growth rate was maintained at 0.025 nm/s, and 20 min growth resulted in a film thickness of 30 nm. For nitridation, pure N2\mathrm{N}_2 gas (99.9999%) was introduced into a radio-frequency (RF) radical source. To create a strong nitriding environment, a custom-designed atomic nitrogen source was operated at 13.56 MHz with an RF power of 400 W. The nitrogen flow rate was set to 2.0 sccm, corresponding to a background nitrogen pressure of 1×10−51 \times10^{-5} Torr. The substrate temperature during growth was monitored using a radiation pyrometer (Japan Sensor), and the growth temperature was 800 °C. The supplied cation ratio (Pr:Ta) was calibrated to 1:1 using EIES and a quartz crystal microbalance equipped in the MBE chamber. The ratio of the resultant film was determined by inductively coupled plasma measurements.

For structural determination, X-ray diffraction (XRD) measurements were performed at room temperature. We used the SAGA Light Source (SAGA-LS) BL15 with a wavelength of 1.00 Å, for the 00l and in-plane XRD measurements (Figure 2 and Figure 3(h)). We also used a Bruker D8 with a Cu Kα\alpha X-ray source (wavelength 1.54 Å) for other crystallographic plane measurements, including symmetric scans and reciprocal space maps (Figure 3(a) - (g) and Figure 4). The X-ray beam from the SAGA-LS has a photon flux at least 100 times higher than that from the Cu source. This high flux is useful for detecting weak diffraction peaks from small crystalline volumes. On the other hand, in terms of intensity stability, the Cu source provides a constant X-ray intensity, whereas the intensity from the SAGA-LS decreases over time. Therefore, the Cu source was used for fitting the measured XRD peaks, since peak intensity is the fitting target. For consistency in the fitting analysis, the lattice parameters presented in this study were obtained from the data measured using the Bruker D8.

Figure 2. XRD symmetric scan in [001]c_c direction of YAO measured in SAGA-LS with wave length of 1.00 Å. The crystalline coherency of PrTaN2_2 in [001] direction is confirmed with the higher order (00ll) peaks up to (006). We also observed the Ta3_3N5_5 (012) and (023) peaks as well as their higher order diffraction peaks, which indicates that our RF radical source achieves the rich nitrogen environment.

Figure 3. XRD symmetric scan aligned in the direction of (a) (101) (χ=45.5∘\chi= 45.5^\circ), (b) (011) (χ=45.4∘\chi= 45.4^\circ), (c) (102) (χ=63.0∘\chi= 63.0^\circ), (d) (103) (χ=72.9∘\chi= 72.9^\circ), (e) (213) (χ=37.0∘\chi= 37.0^\circ), (f) (312) (χ=58.0∘\chi= 58.0^\circ), and (g) (222) (χ=54.8∘\chi= 54.8^\circ) PrTaN2_2 planes. (h) In-plane XRD measurement with χ=0.5∘\chi= 0.5^\circ. The estimated dd spacing are presented in Table 1.

Figure 4. High resolution reciprocal space maps of the PrTaN2_2 thin film around the YAO (103)c_c and YAO (113)c_c peak. Logarithmic scale is used to express the intensity of the diffraction, which is shown as the color bar. The relaxed film is grown on the substrate, and the film and the substrate share the same crystalline axis.

Experimental Results

Novel ternary nitride PrTaN2\mathrm{PrTaN}_2

We have synthesized and identified a novel ternary nitride PrTaN2\mathrm{PrTaN}_2. The film resistivity is higher than 10310^3 Ωm at room temperature, and paramagnetic behavior is observed (see Supporting Information). Our XRD study reveals that the crystal system is orthorhombic, with lattice constants of a=3.97±0.08a = 3.97 \pm0.08 Å, b=4.00±0.08b = 4.00 \pm0.08 Å, and c=4.02±0.01c = 4.02 \pm0.01 Å. The PrTaN2\mathrm{PrTaN}_2 thin film is grown along the cc direction on a YAO (001)c_\mathrm{c} substrate.

A related ternary nitride is LaReN2\mathrm{LaReN}_2 (P4/mmmP4/mmm, a=b=3.97a = b = 3.97 Å, c=3.56c = 3.56 Å). [7] In that system, the perovskite nitride LaReN3\mathrm{LaReN}_3 decomposes at 500-620 °C and is topotactically reduced to LaReN2\mathrm{LaReN}_2. In contrast, PrTaN2\mathrm{PrTaN}_{2} is not obtained via such a reduction process but is directly grown on the substrate. We did not observe the formation of perovskite PrTaN3\mathrm{PrTaN}_{3} within the accessible growth conditions. In the case of PrTaN3\mathrm{PrTaN}_{3}, the valences of Pr and Ta are expected to be +4+4 and +5+5, respectively, whereas both Pr and Ta are considered to be in the +3+3 state in PrTaN2\mathrm{PrTaN}_{2}. The ionization energy of Pr3+\mathrm{Pr}^{3+} is 38.9 eV38.9\,\mathrm{eV} lower than that of Pr4+\mathrm{Pr}^{4+}, [14] which favors the formation of the trivalent state. [12]

Figures 1(a) and (b) show high-angle annular dark-field scanning transmission electron microscopy (HAADF-STEM) images along the [100] and [110] directions of PrTaN2\mathrm{PrTaN}_{2}. Clear atomic ordering is observed in both crystallographic directions. Since ISTEM∝Za2.0I_{\mathrm{STEM}} \propto Z_{a}^{2.0}, [15] where ISTEMI_{\mathrm{STEM}} is the HAADF-STEM intensity and ZaZ_{a} is the atomic number, comparison of the line profiles allows identification of the atomic columns corresponding to Pr (Za=59Z_{a}=59) and Ta (Za=73Z_{a}=73). Figures 1(c) and (d) show the line profiles corresponding to the dashed lines in fig:1a and fig:1b, respectively. The red curve exhibits higher intensity than the blue one, indicating Ta and Pr columns, respectively.

In the HAADF-STEM image along the [100] direction (Fig. 1(a)), the in-plane positions of Pr and Ta are shifted by half a period. In contrast, in the [110] direction (Fig. 1(b)), Pr and Ta are located at the same in-plane positions.

Figures 1(e) and (f) are the fast Fourier transform (FFT) results of Figs. 1(c) and (d). The dominant peaks (α010\alpha_{010} and α1ˉ10\alpha_{\bar{1}10}) of Pr and Ta overlap, indicating that Pr and Ta share the same in-plane periodicity. The frequencies of α010\alpha_{010} and α1ˉ10\alpha_{\bar{1}10} yield the corresponding dd-spacings: d010=1/α010=1/(2.54±0.14 nm−1)=4.07±0.21 A˚d_{010}=1/\alpha_{010}=1/(2.54\pm0.14\,\mathrm{nm}^{-1})=4.07\pm0.21\,\text{\AA}, and d110=1/α1ˉ10=1/(3.52±0.13 nm−1)=2.84±0.10 A˚d_{110}=1/\alpha_{\bar{1}10}=1/(3.52\pm0.13\,\mathrm{nm}^{-1})=2.84\pm0.10\,\text{\AA}. These dd-spacings are in agreement with those obtained from our XRD measurements, as discussed later (see also Table 1).

hklhklExp. (Å)Calc. (Å)
1012.82 ± 0.032.82 ± 0.11
0112.83 ± 0.032.83 ± 0.11
1021.79 ± 0.011.79 ± 0.04
1031.27 ± 0.011.27 ± 0.03
2131.07 ± 0.0041.07 ± 0.03
3121.07 ± 0.0031.07 ± 0.05
2221.16 ± 0.0041.15 ± 0.04
1102.84 ± 0.032.82 ± 0.14

Table 1. Experimental and calculated dd spacing values. When we measured one higher order peaks at least, dd is obtained by Nelson-Riley fitting.[16]

Symmetric scans

Detailed XRD measurements are key to confirming that the obtained phase corresponds to PrTaN2\mathrm{PrTaN}_{2}. Figure 2 shows the θ−2θ\theta-2\theta scan along the YAO [001]c_{\mathrm{c}} direction measured at the SAGA-LS with a wavelength of 1.00 A˚1.00\,\text{\AA}. The PrTaN2(001)\mathrm{PrTaN}_{2}(001) peak and its higher-order diffractions up to (006) are observed, indicating high crystalline coherence along this direction. In addition, Ta3N5\mathrm{Ta}_{3}\mathrm{N}_{5} (012), (023) and their higher order peaks are also observed as secondary phases.

Ta3N5\mathrm{Ta}_{3}\mathrm{N}_{5} is metastable in the Ta-N system compared to TaN and Ta2\mathrm{Ta}_{2}N. The presence of Ta3N5\mathrm{Ta}_{3}\mathrm{N}_{5} as a secondary phase suggests that the growth was carried out under a high effective nitrogen chemical potential. Under such conditions, nitrogen incorporation is enhanced, which may facilitate the formation of nitrogen-rich phases such as PrTaN2\mathrm{PrTaN}_{2} that are not readily obtained under bulk equilibrium synthesis conditions.

To investigate other crystallographic planes, we performed additional symmetric XRD scans with varying tilt angle χ\chi. Figures 3(a)-(g) show the results of symmetric scans corresponding to the (a) (101) (χ=45.5∘\chi=45.5^\circ), (b) (011) (χ=45.4∘\chi=45.4^\circ), (c) (102) (χ=63.0∘\chi=63.0^\circ), (d) (103) (χ=72.9∘\chi=72.9^\circ), (e) (213) (χ=37.0∘\chi=37.0^\circ), (f) (312) (χ=58.0∘\chi=58.0^\circ), and (g) (222) (χ=54.8∘\chi=54.8^\circ) PrTaN2\mathrm{PrTaN}_{2} planes. Figure 3(h) shows the in-plane XRD results measured at SAGA-LS with the wave length of 1.00 A˚1.00\,\text{\AA}. In Figs. 3(a) and (b), we measured the higher order peaks of (101) and (011) planes, which indicates the high crystalline coherency of our film.

The dd spacing values in Figs. 3(a)-(d) are summarized in Table 1. The dd values were determined using the Nelson-Riley fitting procedure [16] when higher-order diffractions were measured. The calculated dd values for an orthorhombic crystal system are given by the following relation:

1d=h2a2+k2b2+l2c2(1)\frac{1}{d}=\sqrt{\frac{h^{2}}{a^{2}}+\frac{k^{2}}{b^{2}}+\frac{l^{2}}{c^{2}}} \tag*{(1)}

For all measured crystallographic planes, the experimental dd values agree with the calculated ones within errors. Also, the φ\varphi scans show the consistent φ\varphi angles between neighboring peaks for (204) and (312) planes (see Supporting Information). These results are consistent with an orthorhombic crystal system, and the estimated lattice constants agree with the experimental data.

In addition, we quantitatively evaluate the monoclinic distortion of the system, namely the deviation of β\beta from 90∘90^\circ. The dd-spacings for a monoclinic system are described as

1d=1sin⁡2β[h2a2+k2b2sin⁡2β+l2c2−2hlcos⁡βac].(2)\frac{1}{d}=\sqrt{\frac{1}{\sin^{2}\beta}\left[\frac{h^{2}}{a^{2}}+\frac{k^{2}}{b^{2}}\sin^{2}\beta+\frac{l^{2}}{c^{2}}-\frac{2hl\cos\beta}{ac}\right]}. \tag*{(2)}
HAADF-STEM images, line intensity profiles, and fast Fourier transform results for PrTaN2

Figure 1. (a,b) High-angle annular dark field scanning transmission electron microscopy (HAADF-STEM) images in the [100] and [110] directions of PrTaN2_2. The inset shows the expanded images with the schematic atomic images of PrTaN2_2. The scale bar corresponds to 1 nm. (c,d) Line intensity profiles of red and blue dashed lines in (a) and (b), respectively. Since the intensity of HAADF-STEM represents the atomic number, we can distinguish the cation positions, which means the red and blue lines represent Ta and Pr. For (c) and (d), Pr and Ta are located in alternate shifts in [001] direction. For the in-plane direction, while Pr and Ta are located half cycle change in (c), they are located same position in (d). (e,f) Fast Fourier transform (FFT) results of (c) and (d). The frequencies of the dominant peaks (α010\alpha_{010}, α1‾10\alpha_{\overline{1}10}) agree with the corresponding d-spacing obtained by our XRD measurements. The harmonic peaks (2α0102\alpha_{010}, 3α0103\alpha_{010} and 2α1‾102\alpha_{\overline{1}10}) are also observed.

Assuming that β\beta deviates from 90∘90^\circ within the uncertainty range of the experimentally determined dd-spacings listed in Table 1, (2) yields a range of 89.9∘<β<90.1∘89.9^\circ< \beta< 90.1^\circ. The deviation of β\beta from 90∘90^\circ is therefore sufficiently small. In other words, treating the system as orthorhombic does not lead to any inconsistency with the experimental results.

Epitaxial relationship and substrate choice

The influence of the substrate is key to understanding the growth mechanism of PrTaN2_2. Figures 4(a) and (b) show reciprocal space maps around the YAO (103)c_c and (113)c_c diffractions. The reciprocal space coordinates (qx,qz)(q_x, q_z) for the diffraction peaks are summarized in Table 2. Here, qxq_x corresponds to q100q_{100} in Figure 4 and to q110q_{110} in Figure 4, while qzq_z corresponds to q001q_{001}.

hklhklMaterialqzq_z (nm−1^{-1})qxq_x (nm−1^{-1})qz/qxq_z/q_x
103PrTaN2_27.49 ± 0.082.48 ± 0.213.02 ± 0.27
103YAlO3_38.09 ± 0.012.69 ± 0.013.00 ± 0.01
113PrTaN2_27.59 ± 0.073.56 ± 0.162.12 ± 0.10
113YAlO3_38.13 ± 0.013.83 ± 0.012.12 ± 0.01

Table 2. Reciprocal space coordinates observed in Fig. 4. qxq_x corresponds to q100q_{100} in Fig. 4(a) and to q110q_{110} in Fig. 4(b), while qzq_z corresponds to q001q_{001}.

The ratios qz/qxq_z/q_x for the (103) and (113) reflections are nearly identical for the PrTaN2_2 film and the YAO substrate, indicating that the film is essentially strain-free. Thus, the lattice constants are not significantly affected by substrate-induced strain. On the other hand, the in-plane crystal orientation is not completely arbitrary but reflects the four-fold symmetry of the YAO substrate. This behavior suggests preferentially oriented growth influenced by the substrate rather than fully coherent epitaxy.

The choice of substrate is an important growth parameter for obtaining ternary nitride thin films. One difficulty in substrate selection is the lack of commercially available nitride substrates with cubic or tetragonal symmetry. Maintaining a high-quality interface between dissimilar materials during crystal growth is generally challenging. So far, a variety of oxide substrates have helped address this issue.

As seen in the RSM measurements, a coherent epitaxial relationship between PrTaN2_2 and the YAO substrate is not established. The pseudo-cubic lattice constant of YAO is 3.71 Å which does not match any characteristic atomic spacing in PrTaN2_2. Oxide substrates such as SrTiO3_3 and KTaO3_3 offer a range of lattice constants around 3.9 Å-4.0 Å, which closely match the aa, bb, and cc lattice constants of PrTaN2_2. However, these substrates are not suitable for growth under the present conditions because their surfaces are not sufficiently resistant to nitridation. The high chemical potential associated with nitrogen radicals and/or ionic nitrogen generated by the RF radical source can degrade the substrate surface by inducing oxygen deficiency.

YAlO3_3 has a higher oxygen vacancy formation energy (∼22\sim22 eV) [17] compared to SrTiO3_3 (∼5.9\sim5.9 eV) [18] and KTaO3_3 (∼5.3\sim5.3 eV). [19] This suggests that YAlO3_3 is more robust against reduction under highly nitriding conditions. Therefore, YAlO3_3 is one of the most suitable choices for ternary nitride thin film growth.

Discussion

Determination of chemical formula and crystal structure

In exploring new materials in thin film form, careful determination of the chemical formula and crystal structure is essential. Even when the observed XRD peaks appear consistent with a given structure, there remains a degree of freedom in assigning the hklhkl indices in terms of integer multiples. In other words, the choice of the unit cell based solely on XRD data is not necessarily unique. To constrain such ambiguity and determine a specific chemical formula and crystal structure, it is necessary to analyze diffraction peaks from multiple crystallographic planes in combination with STEM observations. As mentioned in the Introduction, various ternary nitrides composed of lanthanides and tantalum have been reported. In the present study, we systematically rule out alternative candidate phases based on the combined XRD and STEM analyses.

Pr3_3Ta2_2N6_6 is a Ruddlesden–Popper related phase with tetragonal symmetry (I4/mmmI4/mmm) with a=b=4.06a = b = 4.06 Å and c=19.6c = 19.6 Å.[4] According to the extinction rules for the I4/mmmI4/mmm space group, no diffraction peak is expected in the measured reciprocal space around the (113) reflection This is inconsistent with the experimental observation shown in Figure 4(b).

Perovskite (PrTaN3_3) and the Ruddlesden–Popper phase with n=2n = 2 (Pr2_2TaN4_4) are also possible candidate structures. CeTaN3_3[5] and Ce2_2TaN4_4[8] are reported analogous compounds. However, these possibilities are unlikely based on the observed trivalent state of Pr. Considering that the maximum valence of Ta is +5, Pr is in a tetravalent state in these structures. We also grew isostructural NdTaN2_2 on the YAO substrate (see Supporting Information.) Since Nd and Ta are trivalent, the formation of phases such as PrTaN3_3 and Pr2_2TaN4_4 is unlikely.

Another possible candidate is the brownmillerite phase Pr2_2Ta2_2N5_5. If our film were Pr2_2Ta2_2N5_5, the lattice constants would be estimated as a=5.64a = 5.64 Å, b=5.66b = 5.66 Å, and c=16.1c = 16.1 Å, based on our XRD results. These lattice parameters were obtained by indexing the XRD peaks so that each parameter takes reasonable values compared to those of known brownmillerite compounds. In this scenario, the diffraction peaks observed in the 00l00l scan (Figure 2) can be assigned to the 004 diffraction and its higher-order diffractions (008, 0012, …). The space groups consistent with the extinction rules are F2ddF2dd and FdddFddd. If these space groups were valid, the XRD peak observed in the reciprocal space mapping around YAO(113)c_c (Figure 4(b)) could be indexed as (1 12 1). However, this reflection is forbidden by the extinction rules of both F2ddF2dd and FdddFddd, indicating that the brownmillerite phase is unlikely.

Pr2_2TaN3_3 with orthorhombic symmetry is also a possible candidate. As a similar example, Ce2_2TaN3_3 has been reported.[20] However, this possibility can be ruled out based on the HAADF-STEM measurements. We performed STEM image simulations for Pr2_2TaN3_3 using ReciPro[21] (see Supporting Information). In the [011] direction, the experimental data show an atomic sequence of ⋯–Pr–Ta–Pr–Ta–⋯. In contrast, the simulation exhibits a sequence of ⋯\cdots–Pr–Pr–Ta–Pr–Pr–⋯\cdots. This discrepancy is inconsistent with the experimental observations, indicating that the Pr2TaN3\mathrm{Pr}_{2}\mathrm{TaN}_{3} structure is unlikely.

ScTaN2\mathrm{ScTaN}_{2} has a hexagonal structure (P63/mmcP6_{3}/mmc) and features trivalent Ta, making it a relevant reference polymorph when considering possible crystal structures of PrTaN2\mathrm{PrTaN}_{2}. However, the possibility of a hexagonal structure in the present case is unlikely. Our ϕ\phi scans show no indication of hexagonal symmetry (see Supporting Information). The ϕ\phi scans of the (204) and (312) reflections exhibit fourfold and eightfold peak patterns, respectively. This indicates that the crystal system does not possess sixfold rotational symmetry.

Determination of space group and atomic coordinates

Determining the space group and atomic coordinates is a key challenge in investigating a new material in thin-film form. In general, powder diffraction patterns allow determination of the space group and atomic coordinates through Rietveld analysis. The XRD θ\theta–2θ2\theta scan provides sufficient crystallographic information to determine the crystal structure in powder samples.

In contrast, for single-crystalline thin films, diffraction peaks are distributed in reciprocal space, and only a limited number of crystallographic planes can be measured. Although extinction rules help narrow down possible space groups, they do not always uniquely determine the space group. For example, P222P222 and PmmmPmmm, which belong to the same Laue class, cannot be distinguished solely by extinction rules.[22]

In principle, determining the space group and crystal structure is equivalent to solving the structure factor equations,

Fhkl=∑νfνexp⁡[2πi(hxν+kyν+lzν)],(3)F_{hkl} = \sum_{\nu} f_{\nu}\exp[2\pi i(hx_{\nu}+ky_{\nu}+lz_{\nu})], \tag*{(3)}

where fνf_{\nu} is the scattering factor, and ν\nu represents atomic species. In the case of PrTaN2\mathrm{PrTaN}_{2} with number of formula units per unit cell Z=1Z=1, ν\nu corresponds to Pr, Ta, and two inequivalent nitrogen atoms (denoted as N1 and N2). In this case, one needs to solve the equations with (3×4=)12(3 \times4=)12 parameters for the atomic positions, which is generally impractical to determine directly.

Here, we present a fitting procedure that enables determination of the crystal structure even from thin-film XRD data (fig:5a): (i) Convert the observed XRD peak intensities IobsI_{\mathrm{obs}} into structure factors FobsF_{\mathrm{obs}}. (ii) Select candidate space groups based on extinction rules. (iii) Assign allowed atomic positions according to Wyckoff positions. (iv) Solve an optimization problem to minimize the root-mean-square (RMS) residual between experimental and calculated structure factor values for the observed hklhkl reflections. (v) Compare the RMS values among different space groups and make a decision after screening by chemical bond length. We note that we assumed the smallest translational periodicity compatible with the observed diffraction pattern and adopted a Z=1Z=1 orthorhombic average structure. The reasons why this assumption is justified are discussed later in this section.

For step (i), one needs to account for extrinsic factors that affect the peak intensity. The relationship between IobsI_{\mathrm{obs}} and FobsF_{\mathrm{obs}} is described as[23]

Iobshkl(θ)∝C2(θ)L(θ)Aθ2θ(θ)∣Fobshkl∣2,(4)I_{\mathrm{obs}}^{hkl}(\theta) \propto C^{2}(\theta)L(\theta)A_{\theta2\theta}(\theta)\lvert F_{\mathrm{obs}}^{hkl}\rvert^{2}, \tag*{(4)}

Note that multiplicity and geometrical factors can be neglected in the case of thin films. The polarization factor C2(θ)=(1+cos⁡2θ)/2C^{2}(\theta)=(1+\cos^{2}\theta)/2 represents the angular dependence of the scattering intensity arising from Thomson and Compton scattering. The Lorentz factor L(θ)=(sin⁡(2θ))−1L(\theta)=(\sin(2\theta))^{-1} accounts for the geometrical effect associated with the measurement configuration. The factor Aθ2θ(θ)=1−exp⁡[−μt/(sin⁡θcos⁡χ)]A_{\theta2\theta}(\theta)=1-\exp[-\mu t/(\sin\theta\cos\chi)] describes the attenuation of X-rays in the film, where μ\mu is the linear attenuation coefficient (=1.96×105/m)(=1.96\times10^{5}/\mathrm{m}),[24] tt is the film thickness (=30±0.1 nm)(=30\pm0.1\ \mathrm{nm}), and χ\chi is the tilt angle of the goniometer.

For steps (ii) and (iii), the extinction rules indicate that the candidate orthorhombic space groups are P222P222 (16), P21212P2_{1}2_{1}2 (17), Pmm2Pmm2 (25), and PmmmPmmm (47). In the fitting procedure, one space group is selected from this list, and atomic positions are assigned according to the corresponding Wyckoff positions. The Wyckoff orbits ensure that the symmetry of each hypothetical structure is consistent with the selected space group.

For step (iv), we solved an optimization problem for the atomic positions to minimize the RMS. As an example, in the case of Pmm2Pmm2, the Wyckoff positions can be assigned as Pr (0,yPr,1/2)(0,y_{\mathrm{Pr}},1/2), Ta (1/2,1/4,0)(1/2,1/4,0), N1 (0,yN1,0)(0, y_{\mathrm{N1}}, 0), and N2 (1/2,yN2,1/2)\mathrm{N2}\ (1/2, y_{\mathrm{N2}}, 1/2). In this case, eq. (3) is simplified to include three free fitting parameters (yPr,yN1,yN2)(y_{\mathrm{Pr}}, y_{\mathrm{N1}}, y_{\mathrm{N2}}). In other words, this procedure reduces the number of fitting parameters by utilizing the constraints imposed by Wyckoff positions. When there are no free variables, as in Wyckoff letter 1a (0,0,0)(0,0,0) of P222P222, an atom is simply placed at that position, and no fitting is performed for that site. We note that it is unlikely that atoms occupy general positions. For example, in the case of PmmmPmmm, the multiplicity of the general position is eight (Wyckoff letter 8A). This is physically unlikely because it cannot maintain the stoichiometric ratio of PrTaN2\mathrm{PrTaN}_2, and it would also lead to unrealistic bond lengths (typically <1.0< 1.0 Å).

The positions of Pr and Ta were taken from the STEM images. This procedure further reduces the number of free variables, thereby making the statistical errors in the fitting results sufficiently small. The cation positions determined from STEM were Pr(0.51±0.04,0.53±0.04,0.49±0.01)\mathrm{Pr}(0.51 \pm0.04, 0.53 \pm0.04, 0.49 \pm0.01) relative to Ta(0,0,0)\mathrm{Ta}(0,0,0). Within the uncertainty of the error bars, the only atomic position that Pr could occupy while maintaining the stoichiometry of PrTaN2\mathrm{PrTaN}_2 and satisfying the constraints imposed by the allowed Wyckoff positions was (0.5,0.5,0.5)(0.5,0.5,0.5). Therefore, the actual fitting was performed using Ta(0,0,0)\mathrm{Ta}(0,0,0) and Pr(0.5,0.5,0.5)\mathrm{Pr}(0.5,0.5,0.5).

For step (v), inspection of the RMS values obtained from the fitting revealed that it is difficult to uniquely determine a single structural model solely on the basis of the RMS values, even among the best candidates. Comparing the top five results that correspond to structurally distinguishable candidates, the RMS values ranged only from 0.1735 to 0.1750, indicating that such small differences are insufficient for definitive structure determination. We note that the worst RMS is 44.5 on PmmmPmmm. Therefore, additional screening was performed based on the Pr-N bond distances.

Among the candidates exhibiting nearly optimal RMS values, the nitrogen positions relative to Pr(0.5,0.5,0.5)\mathrm{Pr}(0.5,0.5,0.5) can be broadly classified into the following categories: (1) sharing the aa-axis (i.e., having the same bb and cc coordinates), (2) sharing the bb-axis, (3) sharing the cc-axis, and (4) sharing none of the axes, with N located along the in-plane diagonal directions (e.g., N(0.5,0,0)\mathrm{N}(0.5,0,0) or N(0,0.5,0)\mathrm{N}(0,0.5,0)).

For cases (1)-(3), considering that the lattice constants aa, bb, and cc are all approximately 4.0 Å, the resulting Pr-N distances are about 2.0 Å. To the best of our knowledge, no known compound exhibits such a short Pr-N bond distance. The simple sum of the ionic radii of Pr and N is approximately 2.5-2.8 Å, and the Pr-N distance in rock-salt PrN is 2.58 Å. For these reasons, only category (4) is considered physically plausible. In this case, the Pr-N distance is approximately 4.04.0 Å/2=2.8/\sqrt{2} = 2.8 Å. The space group is estimated to be P222P222 with best RMS = 0.174. The atomic coordinates and the bond lengths are shown in Table 3 and Table 4. Figure 5 shows the crystal structure of PrTaN2\mathrm{PrTaN}_2 using the estimated atomic coordinates.

LabelElementWyckoff positionxxyyzz
PrPr1h (1/2,1/2,1/2)(1/2, 1/2, 1/2)0.50.50.5
TaTa1a (0,0,0)(0, 0, 0)0.00.00.0
N1N1b (1/2,0,0)(1/2, 0, 0)0.50.00.0
N2N1d (0,0,1/2)(0, 0, 1/2)0.00.00.5

Table 3. Optimized atomic coordinates and Wyckoff positions by our fitting procedure (fig:5a). According to our STEM measurements, the cation positions were Pr(0.51±0.04,0.53±0.04,0.49±0.01)(0.51 \pm0.04, 0.53 \pm0.04, 0.49 \pm0.01) relative to Ta(0,0,0)(0,0,0). Among the candidate space groups identified from the extinction rules (P222P222 (16), P21212P2_{1}2_{1}2 (17), Pmm2Pmm2 (25), and PmmmPmmm (47)), the Pr position within this error range is Pr(0.5,0.5,0.5)(0.5,0.5,0.5).

ElementBond length (Å)
Pr - N12.85
Pr - N22.84
Ta - N11.95
Ta - N21.97

Table 4. The chemical bond length between cations (Pr and Ta) and nitrogens (N1 and N2).

Figure 5. (a) Fitting procedure of eq. (3) to the experimental data. To convert the peak intensity IobsI_{\mathrm{obs}} to the structure factor FobsF_{\mathrm{obs}}, we use eq. (4). By using this procedure, we can decrease the number of fitting parameter using Wyckoff positions. (b) Crystal structure of PrTaN2\mathrm{PrTaN}_2 reproduced by the estimated atomic coordinates.

The chosen Wyckoff positions for nitrogen are 1b and 1d, which do not have any free fitting parameter. The obtained structure shows some similarity to LaReN2\mathrm{LaReN}_2; however, a notable difference is that the lattice constants aa, bb, and cc in PrTaN2\mathrm{PrTaN}_2 are nearly identical. Although structural anisotropy is observed along the bb-axis in PrTaN2\mathrm{PrTaN}_2, no corresponding shortening of only the bb-axis lattice constant is found.

The coordination number for Pr and Ta are eight and four, respectively. In ternary nitrides containing Ta, the coordination number of Ta tends to be six, reflecting the Ta high oxidation state (+5). Examples in which Ta has a coordination number of four are rare. CsTaN2\mathrm{CsTaN}_2, in which Ta forms TaN4\mathrm{TaN}_4 tetrahedra, is the only known example. [25] In this context, the possibility that excess nitrogen, lacking long-range order, is incorporated into interstitial sites near Ta cannot be excluded. If the presence of such interstitial nitrogen between the Ta-N planes is assumed, the larger interlayer spacing in PrTaN2\mathrm{PrTaN}_2 compared with LaReN2\mathrm{LaReN}_2 [7] may be understood (PrTaN2\mathrm{PrTaN}_2: 3.97 Å; LaReN2\mathrm{LaReN}_2: 3.56 Å). Similar phenomena, in which excess anions occupying interstitial sites lead to an expansion of the interlayer spacing, are observed in layered oxide compounds. [26, 27, 28] A similar mechanism may therefore be operative in PrTaN2\mathrm{PrTaN}_2.

We also tested lower-symmetry models such as monoclinic P2P2, where nitrogen atoms are no longer constrained to symmetry-equivalent positions and can move more independently. Such models effectively introduce additional crystallographically distinct nitrogen environments while keeping the same translational cell and Z=1Z = 1. However, even with this increased flexibility, the structure-factor fit was not improved significantly (RMS = 0.173). Therefore, the XRD data do not support the need for additional independent nitrogen sites beyond those already present in the higher-symmetry model. Together with the absence of clear superlattice reflections, this indicates that the higher-symmetry Z=1Z = 1 average structure is sufficient to describe the observed diffraction data.

Structure factor analysis of PrTaN2_2

Symmetry Operations and General Coordinates

In this section, we examine in detail the structure factors calculated from the space group obtained by the fitting procedure. The P222P222 space group has primitive lattice centering and three mutually perpendicular twofold rotation axes (2x2_x, 2y2_y, 2z2_z) parallel to the aa, bb, and cc axes, intersecting at the origin (0,0,0)(0, 0, 0).

The general positions generated by these operations for an atom at a general coordinate (x,y,z)(x,y,z) are:

  1. (x,y,z)(x,y,z) — Identity (x,y,z)(x,y,z)

  2. (−x,y,−z)(-x,y,-z) — 2-fold axis along zz: rotation by 180° around (0,0,z)(0, 0, z)

  3. (−x,y,zˉ)(-x,y,\bar{z}) — 2-fold axis along yy: rotation by 180° around (0,y,0)(0, y, 0)

  4. (x,y,zˉ)(x,y,\bar{z}) — 2-fold axis along xx: rotation by 180° around (x,0,0)(x, 0, 0)

General Structure Factor Formula

For an atom sitting in a general position (x,y,z)(x,y,z), its contribution must be summed over all 4 symmetrically equivalent positions generated above. Let us substitute these 4 coordinates into the exponential sum using (3):

Fhkl=f[e2πi(hx+ky+lz)+e2πi(−hx−ky+lz)+e2πi(−hx+ky−lz)+e2πi(hx−ky−lz)](5)F_{hkl}=f\left[e^{2\pi i(hx+ky+lz)}+e^{2\pi i(-hx-ky+lz)}+e^{2\pi i(-hx+ky-lz)}+e^{2\pi i(hx-ky-lz)}\right] \tag*{(5)}

Using grouping terms strategically, we can simplify this expression. Now, we group the terms to separate the zz and −z-z dependencies:

Fhkl=f[e2πilz(e2πi(hx+ky)+e−2πi(hx+ky))+e−2πilz(e2πi(−hx+ky)+e−2πi(−hx+ky))](6)F_{hkl}=f\left[e^{2\pi ilz}\left(e^{2\pi i(hx+ky)}+e^{-2\pi i(hx+ky)}\right)+e^{-2\pi ilz}\left(e^{2\pi i(-hx+ky)}+e^{-2\pi i(-hx+ky)}\right)\right] \tag*{(6)}

Using Euler’s formula (exp⁡(iθ)=cos⁡θ+isin⁡θ\exp(i\theta)=\cos\theta+i\sin\theta) and the identity eiθ+e−iθ=2cos⁡θe^{i\theta}+e^{-i\theta}=2\cos\theta:

Fhkl=2f[e2πilzcos⁡(2π(hx+ky))+e−2πilzcos⁡(2π(−hx+ky))](7)F_{hkl}=2f\left[e^{2\pi ilz}\cos(2\pi(hx+ky))+e^{-2\pi ilz}\cos(2\pi(-hx+ky))\right] \tag*{(7)}

Since cos⁡(−α+β)=cos⁡(α−β)\cos(-\alpha+\beta)=\cos(\alpha-\beta), and expanding the outer exponentials into cosines and sines (e±iθ=cos⁡θ±isin⁡θe^{\pm i\theta}=\cos\theta\pm i\sin\theta), this simplifies to:

Fhkl=4f[cos⁡(2πhx)cos⁡(2πky)cos⁡(2πlz)−isin⁡(2πhx)sin⁡(2πky)sin⁡(2πlz)](8)F_{hkl}=4f\left[\cos(2\pi hx)\cos(2\pi ky)\cos(2\pi lz)-i\sin(2\pi hx)\sin(2\pi ky)\sin(2\pi lz)\right] \tag*{(8)}

Real and Imaginary Parts

Unlike centrosymmetric space groups (like PmmmPmmm) where the imaginary part vanishes because every atom at (x,y,z)(x,y,z) has an inversion counterpart at (xˉ,y,zˉ)(\bar{x},y,\bar{z}), P222P222 is non-centrosymmetric. Therefore, the structure factor is complex and contains both a real part (AA) and an imaginary part (BB):

Fhkl=A+iB(9)F_{hkl} = A + iB \tag*{(9)}

For a general reflection:

A=4∑νfνcos⁡(2πhxν)cos⁡(2πkyν)cos⁡(2πlzν)(10)A = 4\sum_{\nu} f_{\nu}\cos(2\pi h x_{\nu})\cos(2\pi k y_{\nu})\cos(2\pi l z_{\nu}) \tag*{(10)}
B=−4∑νfνsin⁡(2πhxν)sin⁡(2πkyν)sin⁡(2πlzν)(11)B = -4\sum_{\nu} f_{\nu}\sin(2\pi h x_{\nu})\sin(2\pi k y_{\nu})\sin(2\pi l z_{\nu}) \tag*{(11)}

Special Reflections (Systematic Dynamic Absences)

Because P222P222 is a primitive lattice without glide planes or screw axes, there are no systematic absences (extinctions) for general (hkl)(hkl) reflections caused by translational symmetry elements. However, specific projections yield special constraints on the imaginary component:

For (h00)(h00), (0k0)(0k0), and (00l)(00l) reflections: If two of the Miller indices are zero, the imaginary part BB drops to 0 because sin⁡(0)=0\sin(0)=0. For instance, for (h00)(h00):

A=4∑νfνcos⁡(2πhxν),B=0(12)A = 4\sum_{\nu} f_{\nu}\cos(2\pi h x_{\nu}),\qquad B = 0 \tag*{(12)}

Application to Wyckoff Positions (Special Positions)

When atoms sit on special positions, their coordinates simplify significantly, which reduces the number of parameters needed during structure factor fitting (see Table 5). If ones incorporate this into the thin-film intensity profile fitting code, using these explicit geometric simplifications for AA and BB instead of computing a raw exponential matrix significantly accelerates the refinement loop.

Wyckoff LetterMultiplicitySite SymmetryCoordinatesImpact on FhklF_{hkl}
1a to 1d1222(0,0,0)(0,0,0), (0,0,12)(0,0,\frac{1}{2}), etc.B=0B=0 (acts locally centrosymmetric)
2e to 2i22(x,0,0)(x,0,0), (0,y,0)(0,y,0), (0,0,z)(0,0,z), etc.Reduces number of terms in the sum

Table 5. Wyckoff positions of P222P222 and its impact on structure factor FhklF_{hkl}

To calculate the structure factors explicitly for the (111)(111), (222)(222), and (333)(333) reflections of the PrTaN2_2 thin film in the P222P222 space group, the atomic coordinates are:

  • Ta is fixed at the origin: (0,0,0)(0,0,0).

  • Pr is fixed at the body center: (12,12,12)\left(\frac{1}{2},\frac{1}{2},\frac{1}{2}\right).

  • N atoms occupy the category (4) in-plane diagonal positions, putting them at the edge-centers: (12,0,0)\left(\frac{1}{2},0,0\right) and (0,0,12)\left(0,0,\frac{1}{2}\right).

For these specific special coordinates, the imaginary components BB vanish completely because all values contain a sin⁡(0)\sin(0) or sin⁡(π)=0\sin(\pi)=0. The general formula simplifies down to:

Fhkl=∑νfνcos⁡[2π(hxν+kyν+lzν)](13)F_{hkl} = \sum_{\nu} f_{\nu}\cos[2\pi(hx_{\nu}+ky_{\nu}+lz_{\nu})] \tag*{(13)}

Calculation for the (111)(111) Peak. Substitute the atomic positions into the simplified phase summation:

F111=fTacos⁡[2π(0)]+fPrcos⁡[2π(12+12+12)]+fN1cos⁡[2π(12)]+fN2cos⁡[2π(12)](14)F_{111} = f_{\mathrm{Ta}}\cos[2\pi(0)] + f_{\mathrm{Pr}}\cos\left[2\pi\left(\frac{1}{2}+\frac{1}{2}+\frac{1}{2}\right)\right] + f_{\mathrm{N1}}\cos\left[2\pi\left(\frac{1}{2}\right)\right] + f_{\mathrm{N2}}\cos\left[2\pi\left(\frac{1}{2}\right)\right] \tag*{(14)}
=fTacos⁡(0)+fPrcos⁡(3π)+fN1cos⁡(π)+fN2cos⁡(π)(15)= f_{\mathrm{Ta}}\cos(0) + f_{\mathrm{Pr}}\cos(3\pi) + f_{\mathrm{N1}}\cos(\pi) + f_{\mathrm{N2}}\cos(\pi) \tag*{(15)}

Using cos⁡(0)=1\cos(0)=1 and cos⁡(π)=cos⁡(3π)=−1\cos(\pi)=\cos(3\pi)=-1:

F111=fTa−fPr−2fN(16)F_{111} = f_{\mathrm{Ta}} - f_{\mathrm{Pr}} - 2f_{\mathrm{N}} \tag*{(16)}

Since fTa(Za=73)f_{\mathrm{Ta}}(Z_{\mathrm{a}}=73) and fPr(Za=59)f_{\mathrm{Pr}}(Z_{\mathrm{a}}=59) partially cancel each other out, and the nitrogen atoms scatter completely out of phase, ∣F111∣\lvert F_{111}\rvert drops drastically toward zero. This explicitly explains why the (111) peak is systematically absent/unobserved in fig:3g.

Calculation for the (222) Peak Substitute the atomic positions for h=2,k=2,l=2h = 2, k = 2, l = 2:

F222=fTacos⁡[2π(0)]+fPrcos⁡[2π(22+22+22)]+fN1cos⁡[2π(22)]+fN2cos⁡[2π(22)](17)F_{222} = f_{\mathrm{Ta}}\cos[2\pi(0)] + f_{\mathrm{Pr}}\cos\left[2\pi\left(\frac{2}{2}+\frac{2}{2}+\frac{2}{2}\right)\right] + f_{\mathrm{N1}}\cos\left[2\pi\left(\frac{2}{2}\right)\right] + f_{\mathrm{N2}}\cos\left[2\pi\left(\frac{2}{2}\right)\right] \tag*{(17)}
=fTacos⁡(0)+fPrcos⁡(6π)+fN1cos⁡(2π)+fN2cos⁡(2π)(18)= f_{\mathrm{Ta}}\cos(0) + f_{\mathrm{Pr}}\cos(6\pi) + f_{\mathrm{N1}}\cos(2\pi) + f_{\mathrm{N2}}\cos(2\pi) \tag*{(18)}

Using cos⁡(0)=cos⁡(2π)=cos⁡(6π)=1\cos(0) = \cos(2\pi) = \cos(6\pi) = 1:

F222=fTa+fPr+2fN(19)F_{222} = f_{\mathrm{Ta}} + f_{\mathrm{Pr}} + 2f_{\mathrm{N}} \tag*{(19)}

Every single atomic sublattice scatters exactly in phase. This constructive interference yields a massive structure factor magnitude, making the (222) peak highly visible and prominent in Figure 3.

Calculation for the (102) Peak Substitute the atomic positions for h=1,k=0,l=2h = 1, k = 0, l = 2:

F102=fTacos⁡[2π(0)]+fPrcos⁡[2π(12+02+22)]+fN1cos⁡[2π(12)]+fN2cos⁡[2π(22)](20)F_{102} = f_{\mathrm{Ta}}\cos[2\pi(0)] + f_{\mathrm{Pr}}\cos\left[2\pi\left(\frac{1}{2}+\frac{0}{2}+\frac{2}{2}\right)\right] + f_{\mathrm{N1}}\cos\left[2\pi\left(\frac{1}{2}\right)\right] + f_{\mathrm{N2}}\cos\left[2\pi\left(\frac{2}{2}\right)\right] \tag*{(20)}
=fTacos⁡(0)+fPrcos⁡(3π)+fN1cos⁡(π)+fN2cos⁡(2π)(21)= f_{\mathrm{Ta}}\cos(0) + f_{\mathrm{Pr}}\cos(3\pi) + f_{\mathrm{N1}}\cos(\pi) + f_{\mathrm{N2}}\cos(2\pi) \tag*{(21)}

Using cos⁡(0)=cos⁡(2π)=1\cos(0) = \cos(2\pi) = 1 and cos⁡(π)=cos⁡(3π)=−1\cos(\pi) = \cos(3\pi) = -1:

F102=fTa−fPr(22)F_{102} = f_{\mathrm{Ta}} - f_{\mathrm{Pr}} \tag*{(22)}

Since the contributions from N1 and N2 completely cancel each other, the structure factor of (102) is larger than that of (111) (∣F102∣>∣F111∣\lvert F_{102}\rvert> \lvert F_{111}\rvert). As shown in Figure 3, we observed the (102) peak, in contrast to the absence of the (111) peak in Figure 3.

Calculation for the (204) Peak Substitute the atomic positions for h=2,k=0,l=4h = 2, k = 0, l = 4:

F204=fTacos⁡[2π(0)]+fPrcos⁡[2π(22+02+42)]+fN1cos⁡[2π(22)]+fN2cos⁡[2π(42)](23)F_{204} = f_{\mathrm{Ta}}\cos[2\pi(0)] + f_{\mathrm{Pr}}\cos\left[2\pi\left(\frac{2}{2}+\frac{0}{2}+\frac{4}{2}\right)\right] + f_{\mathrm{N1}}\cos\left[2\pi\left(\frac{2}{2}\right)\right] + f_{\mathrm{N2}}\cos\left[2\pi\left(\frac{4}{2}\right)\right] \tag*{(23)}
=fTacos⁡(0)+fPrcos⁡(6π)+fN1cos⁡(2π)+fN2cos⁡(4π)(24)= f_{\mathrm{Ta}}\cos(0) + f_{\mathrm{Pr}}\cos(6\pi) + f_{\mathrm{N1}}\cos(2\pi) + f_{\mathrm{N2}}\cos(4\pi) \tag*{(24)}

Using cos⁡(0)=cos⁡(2π)=cos⁡(4π)=cos⁡(6π)=1\cos(0) = \cos(2\pi) = \cos(4\pi) = \cos(6\pi) = 1:

F204=fTa+fPr+2fN(25)F_{204} = f_{\mathrm{Ta}} + f_{\mathrm{Pr}} + 2f_{\mathrm{N}} \tag*{(25)}

As with the (222) peak, the (204) peak has the large structure factor magnitude, which is consistent with its high intensity observed in Figure 3.

Nitrogen Vacancies

So far, we have assumed full occupancy for all nitrogen sites and have not considered the presence of deficient nitrogen. We first note that introducing nitrogen vacancies into the obtained crystal structure with the refined atomic positions cannot account for the experimental XRD results. This can be demonstrated by comparing the calculated structure factors of the (102) and (204) reflections with the corresponding experimental observations. In the following, we discuss the results by comparing the experimental and calculated values of the structure factor ratio, r=F204/F102r = F_{204}/F_{102}.

Nitrogen defect on N1 site Let x1x_1 (0<x1≤10 < x_1 \le1) denote the occupancy of the N1 site. From eqs. (20) and (23),

F102=fTa−fPr+(1−x1)fN(26)F_{102} = f_{\mathrm{Ta}} - f_{\mathrm{Pr}} + (1 - x_1)f_{\mathrm{N}} \tag*{(26)}
F204=fTa+fPr+(1+x1)fN(27)F_{204} = f_{\mathrm{Ta}} + f_{\mathrm{Pr}} + (1 + x_1)f_{\mathrm{N}} \tag*{(27)}

Then,

r(x1)=fTa+fPr+(1+x1)fNfTa−fPr+(1−x1)fN.(28)r(x_1) = \frac{f_{\mathrm{Ta}} + f_{\mathrm{Pr}} + (1 + x_1)f_{\mathrm{N}}}{f_{\mathrm{Ta}} - f_{\mathrm{Pr}} + (1 - x_1)f_{\mathrm{N}}}. \tag*{(28)}

The derivative of r(x1)r(x_1) with respect to x1x_1 is

∂r∂x1=2fN(fTa+fN)(fTa−fPr+(1−x1)fN)2>0.(29)\frac{\partial r}{\partial x_1} = \frac{2f_{\mathrm{N}}(f_{\mathrm{Ta}} + f_{\mathrm{N}})}{(f_{\mathrm{Ta}} - f_{\mathrm{Pr}} + (1 - x_1)f_{\mathrm{N}})^2} > 0. \tag*{(29)}

Thus, r(x1)r(x_1) is a monotonically increasing function of x1x_1. The experimental value is r=2.8r = 2.8, whereas the calculated value satisfies r(x1)>r(0)=6.0r(x_1) > r(0) = 6.0 for 0<x1≤10 < x_1 \le1. Therefore, nitrogen vacancies at the N1 site cannot reproduce the experimental value.

Nitrogen defect on N2 site Let x2x_2 (0<x2≤10 < x_2 \le1) denote the occupancy of the N2 site. Following the same procedure as for the N1 site,

F102=fTa−fPr−(1−x2)fN(30)F_{102} = f_{\mathrm{Ta}} - f_{\mathrm{Pr}} - (1 - x_2)f_{\mathrm{N}} \tag*{(30)}
F204=fTa+fPr+(1+x2)fN(31)F_{204} = f_{\mathrm{Ta}} + f_{\mathrm{Pr}} + (1 + x_2)f_{\mathrm{N}} \tag*{(31)}

Then,

r(x2)=fTa+fPr+(1+x2)fNfTa−fPr−(1−x2)fN.(32)r(x_2) = \frac{f_{\mathrm{Ta}} + f_{\mathrm{Pr}} + (1 + x_2)f_{\mathrm{N}}}{f_{\mathrm{Ta}} - f_{\mathrm{Pr}} - (1 - x_2)f_{\mathrm{N}}}. \tag*{(32)}

The derivative of r(x2)r(x_2) with respect to x2x_2 is

∂r∂x2=−2fN(fPr+fN)(fTa−fPr−(1−x2)fN)2<0.(33)\frac{\partial r}{\partial x_2} = \frac{-2f_{\mathrm{N}}(f_{\mathrm{Pr}} + f_{\mathrm{N}})}{(f_{\mathrm{Ta}} - f_{\mathrm{Pr}} - (1 - x_2)f_{\mathrm{N}})^2} < 0. \tag*{(33)}

Thus, r(x2)r(x_2) is a monotonically decreasing function of x2x_2. The experimental value is r=2.8r = 2.8, whereas the calculated value satisfies r(x2)≥r(1)=7.7r(x_2) \ge r(1) = 7.7 for 0<x2≤10 < x_2 \le1. Therefore, nitrogen vacancies at the N2 site also cannot reproduce the experimental value.

Overall, introducing nitrogen vacancies cannot account for the experimentally observed value of rr. One possible way to reconcile this discrepancy is to introduce excess nitrogen at interstitial sites. However, there are too many possible interstitial sites to establish a unique structural model. Determining the positions of the excess nitrogen atoms will require further structural studies, such as single-crystal neutron diffraction measurements on PrTaN2_2.

Conclusion

We grew a novel ternary nitride PrTaN2_2 thin film on a YAO substrate using a custom-designed molecular beam epitaxy system. Detailed STEM and XRD measurements reveal that the crystal system is orthorhombic. The estimated lattice constants are consistent with the XRD experimental data. Reciprocal space map measurements indicate that the film is essentially strain-free. In selecting substrates, not only lattice mismatch but also surface stability under nitridation conditions should be considered.

For a novel material discovered in thin-film form, determining the chemical formula and crystal structure remains a significant challenge. We systematically ruled out alternative candidate phases in the Pr-Ta-N system. To determine the crystal structure, we developed a fitting procedure based on structure factors. By utilizing constraints from Wyckoff positions, the number of free parameters in fitting Eq. (3) to the experimental data can be significantly reduced. Using this approach, we determined the space group P222P222 and atomic coordinates of PrTaN2_2. This study provides a pathway for the exploration of new ternary nitride thin films.

References

  1. [1]Sun, W.; others Nat. Mater. 2019, 18, 732–739.
  2. [2]Niewa, R.; DiSalvo, F. J. Chem. Mater. 1998, 10, 2733–2752.
  3. [3]DiSalvo, F. J.; Clarke, S. J. Curr. Opin. Solid State Mater. Sci. 1996, 1, 241–249.
  4. [4]Cario, L.; Gál, Z. A.; Braun, T. P.; DiSalvo, F. J.; Blaschkowski, B.; Meyer, H.-J. J. Sol. Sta. Chem. 2001, 162, 90–95.
  5. [5]Choi, S. et al. Sci. Adv. 2025, 11, eadu6698.
  6. [6]Talley, K. R.; Perkins, C. L.; Diercks, D. R.; Brennecka, G. L.; Zakutayev, A. Science 2021, 374, 1488–1491.
  7. [7]Kloß, S. D.; Weidemann, M. L.; Attfield, J. P. Angew. Chem. Int. Ed. 2021, 60, 22260–22264.
  8. [8]Weidemann, M.; Werhahn, D.; Mayer, C.; Kläger, S.; Ritter, C.; Manuel, P.; Attfield, J. P.; Kloß, S. D. Nat. Chem. 2024, 1723–1731.
  9. [9]Zakutayev, A.; Jankousky, M.; Wolf, L.; Feng, Y.; Rom, C. L.; Bauers, S. R.; Borkiewicz, O.; LaVan, D. A.; Smaha, R. W.; Stevanovic, V. Nat. Synth. 2024, 3, 1471–1480.
  10. [10]Grosso, B. F.; Davies, D. W.; Zhu, B.; Walsh, A.; Scanlon, D. O. Chemical Science 2023, 14, 9175–9185.
  11. [11]Flores-Livas, J. A.; Sarmiento-Pérez, R.; Botti, S.; Goedecker, S.; Marques, M. A. J. Phys. Mater. 2019, 2, 025003.
  12. [12]Sarmiento-Pérez, R.; Cerqueira, T. F. T.; Körbel, S.; Botti, S.; Marques, M. A. L. Chem. Mater. 2015, 27, 5957–5963.
  13. [13]Yamamoto, H.; Krockenberger, Y.; Naito, M. J. Cryst. Growth 2013, 378, 184–188.
  14. [14]Kramida, A.; Yu. Ralchenko; Reader, J.; and NIST ASD Team NIST Atomic Spectra Database (ver. 5.12), [Online]. Available: https://physics.nist.gov/asd [2026, March 30]. National Institute of Standards and Technology, Gaithersburg, MD., 2024.
  15. [15]Pennycook, S. J. Characterization of Materials; Wiley, 2012; pp 1–29.
  16. [16]Nelson, J. B.; Riley, D. P. Proc. Phys. Soc. 1945, 57, 160–177.
  17. [17]Fu, M.; Liu, T.; Lu, X.; Li, J.; Ma, Z. Computational Materials Science 2018, 141, 127–132.
  18. [18]Rusevich, L. L.; Tyunina, M.; Kotomin, E. A.; Nepomniashchaia, N.; Dejneka, A. Sci. Rep. 2021, 11, 23341.
  19. [19]Choi, M.; Oba, F.; Tanaka, I. Phys. Rev. B 2011, 83, 214107.
  20. [20]Broll, S.; Jeitschko, W. Z. Naturforsch. 1995, 50, 905–912.
  21. [21]Seto, Y.; Ohtsuka, M. J. Appl. Cryst. 2022, 55, 397–410.
  22. [22]Looijenga-Vos, A.; Buerger, M. J. International Tables for Crystallography; International Union of Crystallography, 2006; pp 44–54.
  23. [23]Birkholz, M.; Genzel, C. Thin Film Analysis by X-Ray Scattering; Wiley, 2005; pp 239–295.DOI
  24. [24]Hubbell, J.; Seltzer, S. Tables of X-Ray Mass Attenuation Coefficients and Mass Energy-Absorption Coefficients (version 1.4). [Online] Available: http://physics.nist.gov/xcomandi[2026, March 30]. National Institute of Standards and Technology, Gaithersburg, MD., 2004.
  25. [25]Cordes, N.; Niklaus, R.; Schnick, W. Cryst. Growth Des. 2019, 19, 3484–3490.
  26. [26]Adachi, H.; Satoh, T.; Ichikawa, Y.; Setsune, K.; Wasa, K. Physica C 1992, 196, 14–16.
  27. [27]Mercey, B.; Gupta, A.; Hervieu, M.; Raveau, B. J. Solid State Chem. 1995, 116, 300–306.
  28. [28]Tomaschko, J.; Leca, V.; Selistrovski, T.; Diebold, S.; Jochum, J.; Kleiner, R.; Koelle, D. Phys. Rev. B 2012, 85, 024519.

Paper details

vlnc:W_kvwm32a3
Version
v1 · latest
Published
Added
License
CC BY 4.0
Usage

views · 0

downloads · 0

A view counts once per browser per day, a download each time the PDF is requested.

  • Physics and Astronomy