betaFeedback

WorksPhysics and Astronomy

Unconventional Charge-density-wave Order in a Dilute d-band Semiconductor

Abstract

Electron-lattice coupling effects in low dimensional materials give rise to charge density wave (CDW) order and phase transitions. These phenomena are critical ingredients for superconductivity and predominantly occur in metallic model systems such as doped cuprates, transition metal dichalcogenides, and more recently, in Kagome lattice materials. However, CDW in semiconducting systems, specifically at the limit of low carrier concentration region, is uncommon. Here, we combine electrical transport, synchrotron X-ray diffraction and optical spectroscopy to discover CDW order in a quasi-one-dimensional (1D), dilute d-band semiconductor, BaTiS3, which suggests the existence of strong electron-phonon coupling. The CDW state further undergoes an unusual transition featuring a sharp increase in carrier mobility. Our work establishes BaTiS3 as a unique platform to study the CDW physics in the dilute filling limit to explore novel electronic phases.

Introduction and main text

Charge density wave (CDW) is a periodic modulation of electron density, which is accompanied by periodic lattice distortions and is often observed in low-dimensional metals or semimetals[1, 14, 15]. The discovery of unconventional CDW order in strongly correlated superconductors such as doped cuprates[5, 6, 16, 17] continues to challenge and expand our understanding of CDW physics and its connection to superconductivity. Recently, there is a growing interest in semiconducting materials that show CDW transitions, such as 1T1T-TiSe2\mathrm{TiSe}_2[18, 19], Ta2NiSe5\mathrm{Ta}_2\mathrm{NiSe}_5[20, 21], and EuTe4\mathrm{EuTe}_4[22, 23], whose origin presumably go beyond the classic Peierls’ picture. They show phenomena such as electronic carrier-type switching[24], toroidal dipolar structures[21, 25], and unconventional hysteretic transitions[22], and this has led to a vigorous debate over the mechanism of these CDW transitions[22, 26]. Here, we report the discovery of unconventional CDW order and phase transitions in a non-degenerate semiconductor, BaTiS3\mathrm{BaTiS}_3, which broadens the realm of CDW physics, especially in semiconducting materials. Upon cooling, we observe, first an increase and then a decrease of electrical resistivity as well as the activation energy across two phase transitions, which signals the emergence and suppression of the CDW state, respectively. Combining single-crystal X-ray diffraction (XRD) and optical probes, we provide direct experimental evidence of CDW order in the system and track down its evolution in both electronic and lattice degrees of freedom. Our experiments establish semiconducting BaTiS3\mathrm{BaTiS}_3 as a new model system to study rich electronic phases and phase transitions associated with CDW in dilute filling.

Transport signatures of CDW phase transitions in BaTiS3\mathrm{BaTiS}_3

Quasi-one-dimensional (quasi-1D) chalcogenide, BaTiS3\mathrm{BaTiS}_3, is a small bandgap semiconductor (Eg∼0.3 eVE_g \sim0.3\ \mathrm{eV}) with a hexagonal crystal structure composed of 1D chains of TiS6\mathrm{TiS}_6 octahedra, stacked between Ba chains (Figure 1a). Recently, unusual physical properties such as giant optical anisotropy[27] and abnormal glass-like thermal transport properties[28] were reported in this material, which promotes questions over its electronic properties. We performed electrical transport measurements on bulk single crystals of BaTiS3\mathrm{BaTiS_3} along the chain axis (cc-axis) (Figure 1b). Here, we identify two different phase transitions from their hysteretic transport behavior. The striking feature of these transitions is their non-monotonic temperature dependence of resistivity. On cooling from room temperature, the resistivity increases, and undergoes a phase transition at 240 K that we refer to as Transition II. On further cooling, it continuous to increase till 150 K, after which it undergoes another transition featuring a sharp drop in resistivity, which we call Transition I. The thermal activation energy, ΔE\Delta E, across the transitions (ΔE≅δ(ln⁡(R))/δ(1/kBT)\Delta E \cong\delta(\ln(R))/\delta(1/k_{\mathrm{B}}T)) shows a clear increase from 75 meV to 153 meV at Transition II and then, a drop to 85 meV at Transition I during cooling cycle (Extended Data Figure 6). The Transition II (240-260 K) hints at the emergence of a CDW state from a high temperature semiconducting phase; while at Transition I (150-190 K), the electrical resistivity reduces dramatically by about an order of magnitude upon cooling and the hysteretic transition window spans over 40 K. This transition towards a more conductive state and the low temperature suppression of CDW order are rather unique among known CDW systems and points to an unconventional origin.

Signature of phase transitions from electrical transport measurements

Figure 1. Signature of phase transitions from electrical transport measurements. a, Room temperature P63cmP6_{3}cm structure of BaTiS3_{3}, showing hexagonal symmetry. b, Illustration of representative temperature dependent electrical resistivity of BaTiS3_{3} crystal along c-axis. Abrupt and hysteric jumps in resistance are shown near 150–190 K (Transition I), and 240–260 K (Transition II). Inset shows optical microscopic image of a BaTiS3_{3} device used for Hall measurements. c, Temperature dependence of the mobility, μ\mu, and carrier concentration, nn, of the dominant carrier, extracted from Hall measurements during a warming cycle.

Thermal activation energy analysis plot showing ln (R) versus $1/k_{\mathrm{B}}T$ with activation energies of 75 meV, 153 meV, and 85 meV

Extended Data Figure 6. Thermal activation energy analysis of BaTiS3_3 transport data presented in Figure 1b. The activation energy is obtained from ΔE=δ(ln⁡(R))δ(1/kBT)\Delta E = \frac{\delta(\ln(R))}{\delta(1/k_{\mathrm{B}}T)} in the linear region. The extracted activation energy before and after Transition II, as well as after Transition I is 75 meV, 153 meV, and 85 meV, respectively.

To further understand these observations, we performed Hall measurements to study the evolution of carrier concentration and mobility across both the phase transitions (Figure 1c). At room temperature, the electron concentration is ∼1.1×1018 cm−3\sim1.1 \times10^{18}\ \mathrm{cm}^{-3}, and it decreases monotonically as temperature is lowered (n<1015 cm−3n < 10^{15}\ \mathrm{cm}^{-3} at 100 K). We did not observe any change in the carrier type across the transitions. These observations confirm the non-degenerate nature of BaTiS3\mathrm{BaTiS_3}, which possesses one of the lowest carrier densities among reported CDW compounds. Further, the Hall mobility is found to increase by about one order of magnitude below Transition I, which is directly associated with observed drop in electrical resistance, suggesting the formation of a higher mobility ground state from the CDW phase. All these transport observations are consistent with two phase transitions that lead to a sequence of electronic phases in BaTiS3_3, starting from a high-temperature semiconducting phase that transitions to a CDW phase at intermediate temperatures, and finally to a unique higher mobility phase at low temperatures.

Evidence for CDW evolution revealed by structural characterization

The superlattice reflections in a diffraction pattern is one of the direct experimental evidences for CDW, which indicates periodic lattice distortions associated with the charge modulation[24, 29, 30]. We performed synchrotron XRD at three different temperatures to track the structural changes during phase transitions. Fig. 2a shows the corresponding precession map projected onto the hk2hk2 reciprocal plane. A hexagonal array of reflection spots is observed at room temperature consistent with P63cmP6_3cm space group (a=b=11.7a=b=11.7 Å, c=5.83c=5.83 Å). At 220 K, additional superlattice reflections appear at h+1/2h+1/2 k+1/2k+1/2 2 in the precession image, which signals a change in the periodicity of the lattice (a=b=23.3a=b=23.3 Å, c=5.84c=5.84 Å) associated with Transition II (P63cmP6_3cm to P3c1P3c1). The intensities of these 2×22 \times2 commensurate superstructure reflections are two orders of magnitude lower than that of the primary reflections and are signatures of the formation of CDW order below Transition II. The unit cell doubling takes place in the aa-bb plane, rather than along the chain cc-axis, which is usually the case in other classic quasi-1D CDW systems such as NbSe3_3[31] and BaVS3_3[32]. On further lowering the temperature to 130 K, the superlattice peaks disappeared and a new set of reflections associated with a smaller 23×23\frac{2}{\sqrt{3}} \times\frac{2}{\sqrt{3}} unit cell emerged (a=b=13.4a=b=13.4 Å, c=5.82c=5.82 Å), which indicates the suppression of the CDW via Transition I (P3c1P3c1 to P21P2_1). The low temperature space group P21P2_{1} is not a subgroup of P3c1P3c1, and we have observed the large thermal hysteresis from transport measurements, both of which lead us to the conclusion that the Transition I is a first-order transition.

To further gain insights into the evolution of electronic structures in BaTiS3\mathrm{BaTiS}_{3} across these transitions, we calculated the electronic band structure of the three phases, based on refined crystal structures from XRD, using density-functional theory (DFT) (Extended Data Figure 9). As temperature is lowered, the bandgap of the system increases from 0.26 eV to 0.3 eV at Transition II and then drops to 0.15 eV across Transition I, which qualitatively agrees with the evolution of thermal activation barrier from Arrhenius analysis of transport data (Extended Data Figure 6).

DFT-calculated electronic band structures of different phases of BaTiS3

Extended Data Figure 9. DFT-calculated electronic band structures of different phases of BaTiS3_3. a, P63cmP6_3cm, b, P3c1P3c1, and c, P21P2_1. The contribution of Ti dd-states and S pp-states to the band structure are highlighted with blue and red colors, respectively. The band gap (EgE_g) calculated at the PBE level are labeled below.

Optical characterization of BaTiS3\mathrm{BaTiS}_{3}

Raman spectroscopy is a sensitive probe to detect symmetry changes in the lattice[33], and to study phase transitions[34, 35]. To complement the structural analysis with XRD, we carried out temperature-dependent Raman scattering measurements on BaTiS3\mathrm{BaTiS}_{3}, as presented in Fig. 3a. A clear change in structure with the emergence of 20 new phonon modes near ~170 K (Transition I) was observed, while the effect from Transition II is subtle. The 23×23\frac{2}{\sqrt{3}} \times\frac{2}{\sqrt{3}} lattice reconstruction observed from XRD coincides with the emergence of new zone-folded Raman modes (See Methods). Furthermore, upon heating, we observe the softening of the mode near 35 cm−1\mathrm{cm}^{-1} with an increase in its bandwidth (Fig. 3b). This mode survives until at least 165 K, above which it gets buried under Rayleigh peak. Since the amount of softening is substantial and its energy is relatively small (35 cm−1\mathrm{cm}^{-1}), we identify it as the soft mode of Transition I.

Given the knowledge of the electronic and structural degrees of freedom in these transitions, we seek to examine the interaction between these two subsystems. Optical transient reflectivity (TR) measurements provide insights into the nature of electron-phonon coupling[36, 37] and the changes in the energy gap. In this experimental scheme, an ultrashort near-infrared pulse (1.63 eV) generates electron-hole pairs in BaTiS3\mathrm{BaTiS}_{3}, which consequently release this energy via relaxation mechanisms such as electron-electron and electron-phonon interactions in ultrafast timescales; the TR traces possess the fingerprints of these relaxation mechanisms. By analyzing the electronic decay rate in TR, and its temperature evolution (Fig. 3c), we observe a critical divergence of relaxation time near 240 K (Transition II). The critical slowing down usually indicates the opening of an energy gap and is associated with a flattening of the Landau free energy at a second-order transition point, which are consistent with a CDW phase transition[37, 38].

Discussion

CDW transitions in other ternary hexagonal chalcogenides such as BaVS3\mathrm{BaVS}_{3} and BaNbS3\mathrm{BaNbS}_{3} are well documented in the literature[39, 40, 41]. These compounds are metallic with a d1d^{1} electronic configuration, whereas stoichiometric BaTiS3\mathrm{BaTiS}_{3} has a d0d^{0} configuration with a nominally empty conduction band. The carrier concentrations measured by Hall measurements in BaTiS3\mathrm{BaTiS}_{3} is too low to support a Peierls-type CDW transition. Another surprising observation is the two-dimensionality of the lattice ordering vector that lies in the aa-bb plane (Fig. 2), whereas BaTiS3\mathrm{BaTiS}_{3} consists of 1D chains of face-sharing TiS6\mathrm{TiS}_{6} octahedra and shows giant uniaxial optical anisotropy[27] at room temperature. To understand the underlying electronic anisotropy, we performed in-plane conductivity anisotropy measurements on BaTiS3\mathrm{BaTiS}_{3} (Extended Data Figure 7). The measured anisotropy in resistivity (ρa/ρc\rho_{a}/\rho_{c}) was ~ 4 based on Montgomery analysis[42, 43], which is relatively small compared to other model quasi-1D metallic CDW systems like NbSe3\mathrm{NbSe}_{3} (ρa/ρc\rho_{a}/\rho_{c} ~ 15-20)[44] and (TaSe4)2I(\mathrm{TaSe}_{4})_{2}\mathrm{I} (ρa/ρc>200)(\rho_a/\rho_c > 200) [45]. This suggests an important role of interchain coupling in stabilizing the CDW phase.

Two-panel plot showing in-plane electrical conductivity anisotropy analysis: panel a plots resistance versus temperature for cooling and warming measurements of $R_{\mathrm{cc}}$ and $R_{\mathrm{aa}}$; panel b plots $R_{\mathrm{aa}}/R_{\mathrm{cc}}$ versus $B_{\alpha,k}$ with the Montgomery conformal mapping curve and van der Pauw measurement geometry inset

Extended Data Figure 7. In-plane electrical conductivity anisotropy analysis using Montgomery method. a, Measured van der Pauw resistance RaaR_{\mathrm{aa}} and RccR_{\mathrm{cc}} as a function of temperature. The transport data was collected from a BaTiS3_3 platelet device with van der Pauw geometry (l=w=20l = w = 20 μm), as shown in the inset of Fig. S7 b. b, The conformal mapping function that uniquely maps the ratio Raa/RccR_{\mathrm{aa}}/R_{\mathrm{cc}} to Bα,kB_{\alpha,k}, which is later used to calculate the anisotropy ρa/ρc\rho_{\mathrm{a}}/\rho_{\mathrm{c}}.

One of the proposed mechanisms for archetypical d0d^{0}-type semiconducting systems such as 1T1T-TiSe2\mathrm{TiSe}_{2}[18] and Ta2NiSe5\mathrm{Ta}_{2}\mathrm{NiSe}_{5}[20] is the excitonic insulator state. As we did not observe any carrier type switching in BaTiS3\mathrm{BaTiS}_{3} from Hall measurements, we can rule out the role of electron-hole coupling in stabilizing the observed CDW order. Detailed analysis of the single crystal XRD at room temperature reveals anomalous Ti-displacements at room temperature with an antipolar structure, similar to 1T1T-TiSe2\mathrm{TiSe}_{2}[25] and Ta2NiSe5\mathrm{Ta}_{2}\mathrm{NiSe}_{5}[21]. Hence, it is likely that the CDW transition is lattice driven with the dimerization of this underlying antipolar structure. Further studies are necessary to probe the evolution of phonon dispersion across the transitions to confirm the role of lattice as the driving force.

Moreover, BaTiS3\mathrm{BaTiS}_{3} is a narrow bandgap semiconductor with non-degenerate, dilute concentration of electrons. Hence, the role of electron-electron interaction could be non-trivial unlike most metallic or semi-metallic CDW systems. One way to evaluate the electron correlation effects in a material is by calculating the dimensionless parameter rs=143πn3(4πεℏ2mbe2)r_s = \sqrt[3]{\frac{1}{\frac{4}{3}\pi n}}\left(\frac{4\pi\varepsilon\hbar^2}{m_b e^2}\right), defined by the ratio of Wigner-sphere radius (dominated by electron-electron interaction) to Bohr radius for a 3D electronic system[46]. Using the experimentally measured carrier concentration nn and calculated band effective mass mbm_b and static dielectric constant ε\varepsilon from DFT, we obtained a rsr_s value of BTS close to 4.4 at 200 K (n=8.2×1016 cm−3n = 8.2 \times10^{16}\ \mathrm{cm}^{-3}), and it further reaches 18.5 at 90 K (n=1.7×1014 cm−3n = 1.7 \times10^{14}\ \mathrm{cm}^{-3}). As systems with rsr_s values ∼100\sim100 are considered to be in the strongly correlated region[46], one cannot rule out the role of electronic correlations in BaTiS3\mathrm{BaTiS}_{3} in effecting these transitions. Further, a cooperative mechanism with electron-lattice and electron-electron interactions could also lead to the phase transitions in BaTiS3\mathrm{BaTiS}_{3}.

To fully understand the origin of these transitions, we need to probe the electronic structure and phonon dispersion across the two transitions. Further studies on the response of the phase transitions in BaTiS3_{3} to external fields such as pressure, strain, and doping, and whether electronic phases such as superconductivity can emerge in BaTiS3_{3} are also of interest. These approaches may also provide a pathway to push the system further into the strongly correlated regime and/or even achieve novel polaronic correlated electronic phases[47, 48] by manipulating the competition between electron-lattice and electron-electron interactions. Our experimental findings of CDW order with novel phase transitions expand the realm of CDW physics to semiconducting materials with dilute filling and establish BaTiS3_{3} as a unique platform featuring a rich phase diagram to study electron correlation and electron-lattice interactions.

Acknowledgements

This work was supported by an ARO MURI with award number W911NF-21-1-0327, an ARO grant with award number W911NF-19-1-0137 and NSF grants with award numbers DMR-2122070 and 2122071. The work at MIT in Gedik Group (B.Y., E.E. and N.G.) was supported by the US Department of Energy, BES DMSE and Gordon and Betty Moore Foundation’s EPiQS Initiative Grant GBMF9459. Work at MIT in the Photon Scattering Group (Q.S., C.A.O. and R.C.) was supported by the National Science Foundation under Grant No. 1751739. J.M., S.O. and J.-H.C. acknowledge the support of the David and Lucile Packard Foundation and the State of Washington funded Clean Energy Institute. This research used resources of the Advanced Light Source, which is a DOE Office of Science User Facility under contract No. DE-AC02-05CH11231. We acknowledge the use of computational resources from the Extreme Science and Engineering Discovery Environment (XSEDE), which is supported by NSF grant number ACI-1548562. A portion of this research used resources at the Spallation Neutron Source, a DOE Office of Science User Facility operated by the Oak Ridge National Laboratory. We thank Alfred Zong and Edoardo Baldini for fruitful discussions.

Author contributions

H.C. and J.R. conceived the idea and designed the experiments. N.G. and R.C. supervised the Raman and transient reflectivity studies. H.C. fabricated the devices and performed electrical transport measurements. J.M., S.O., and G.G. contributed to the transport measurements. B.Z., S.J.T., and B.C.C. performed single crystal X-ray diffraction measurements. B.I., Q.S., and C.A.O. carried out Raman measurements. B.I. and E.E. performed transient reflectivity measurements. G.Y.J., G.R., and J.L. contributed to the theoretical calculations under the supervision of R.M. S.S. and E.S. performed STS studies under the supervision of A.N.P. S.N. and B.Z. grew BaTiS3BaTiS_{3} crystals. All authors discussed the results. H.C., B.I., and J.R. wrote the manuscript with input from all other authors.

Additional information

Competing financial interests

Evidence for CDW order evolution via single crystal XRD, including precession images, X-ray intensity cuts, unit cell evolution, and electronic phases and phase transitions

Figure 2. Evidence for CDW order evolution via single crystal XRD. a, Precession images from single-crystal X-ray diffraction measurements along hk2 projection at 298 K, 220 K and 130 K. b, X-ray intensity cut along the direction as indicated in Fig. 2a. c, Illustration of unit cell evolution of BaTiS3_3 at different temperatures. d, Summary of electronic phases and phase transitions in BaTiS3_3.

Optical characterization of phase transitions

Figure 3. a, Temperature dependent Raman spectra (parallel channel) of BaTiS3_3. The spectrum shows a marked change upon cooling below ∼170\sim170 K (Transition I), with more than 20 new Raman modes emerging. b, Mode hardening of the “Soft mode” near 35 cm−1^{-1}. The bandwidth (in blue) widens upon heating across the transition temperature. c, Transient reflectivity trace at three different temperatures (80 K, 250 K and 290 K). The relaxation times of excited carriers are extracted by fitting with a single exponential function plus a constant. The inset shows temperature dependence of relaxation times. Around ∼240\sim240 K (Transition II), decay time diverges from both sides of this temperature.

Methods

Crystal growth and room temperature characterization

Single crystals of BaTiS3\mathrm{BaTiS}_{3} were grown by chemical vapor transport method as reported elsewhere[1]. Extended Data Fig. 1 illustrates different morphologies of the obtained crystals with a- and c-axis in plane. Single-crystal diffraction performed at room temperature shows no substantial differences structurally between them (Extended Data Table 4). Needle-like crystals with well-defined c-axis are usually picked for transport measurements. For in-plane transport anisotropy measurements, as well as all temperature-dependent optical and single-crystal XRD characterization in this manuscript, we used BTS platelet samples.

Scanning tunneling microscopy (STM) / scanning tunneling spectroscopy (STS) measurements were performed on freshly cleaved surface from a needle sample at room temperature (Extended Data Fig. 2). Surface morphology scan clearly resolves the crystal surface with RMS roughness less than 0.5 nm, and dI/dV\mathrm{d}I/\mathrm{d}V spectra indicates a semiconducting feature with ∼0.3 eV\sim0.3\ \mathrm{eV} bandgap, which is consistent with both the reported optical absorption spectra[1] and DFT calculations.

Device fabrication

As-grown BTS crystals (1010-20 μm20\ \mu\mathrm{m} thick) are embedded in a polymeric media to planarize the top surface such that regular lithography and metallization methods can be readily applied, as illustrated in Extended Data Fig. 3a. Low stress polyimide with coefficient of thermal expansion (CTE) ∼3×10−6 K−1\sim3 \times10^{-6}\ \mathrm{K}^{-1} is chosen to minimize the effect of thermal contraction on transport behaviors at low temperatures. Ohmic contacts to BaTiS3\mathrm{BaTiS}_{3} crystals were fabricated using photolithography, followed by e-beam evaporation of Ti / Au (3 / 300 nm) and lift-off. An SF6\mathrm{SF}_{6} / Ar RIE treatment step (10 / 40 sccm, 100 W, 100 mTorr, 1 min) was applied right before metal deposition to remove surface oxides and further reduce the contact resistance. Optical images of BTS devices are shown in Extended Data Fig. 3b and 3c.

Electrical transport measurements and analysis

Regular transport measurements were carried out in a JANIS 10 K closed-cycle cryostat from 100 K to 300 K. Standard low-frequency (f=17f = 17 Hz) AC lock-in techniques (Stanford Research SR830) were used to measure sample resistance in four-probe geometry, with an excitation current of about 100 nA. Qualitatively reproducible transport behavior showing two characteristic phase transitions was obtained from various devices, different cooling rate, as shown in Extended Data Figure 4. Voltage-tuned transport measurements were performed with DC filed ranging from 0.9 V / mm to 15.1 V / mm, and the transition temperatures of Transition II were found to be reduced as DC bias increases (Extended Data Figure 5).

a: normalized resistance $R(T)/R(300\ \mathrm{K})$ versus Temperature (K), with legend Sample A, Sample B, Sample C; b: Resistance (Ohm) versus Temperature (K), with legend 2 K/min, 5 K/min

Extended Data Figure 4. Reproducible transport measurements. a, Temperature-dependent electrical resistance (normalized by RR (300 K)) measured from three different BaTiS3_3 devices. The transport behavior is qualitatively consistent with each other. b, Cooling rate-dependent transport on BaTiS3_3. Neither of the transitions are suppressed or altered using cooling rate up to 5 K/min.

Two-panel plot. Panel a: Resistivity (Ohm·cm) versus Temperature (K), with DC Bias (V/mm) legend values 0.9, 1.9, 3.8, 5.7, 7.6, 9.5, 11.3, and 15.1; logarithmic resistivity ticks from 10⁻¹ to 10⁴. Panel b: T_C (K) versus DC Bias (V/mm), showing cooling and warming curves.

Extended Data Figure 5. Voltage-tuned transport behavior. a, Temperature-dependent electrical resistivity of BaTiS3_3 crystal along c-axis measured at different DC voltage bias. b, Extracted transition temperature TC_\mathrm{C} of Transition II (∼\sim250 K) as a function of DC bias for both cooling and warming cycles.

In-plane conductivity anisotropy was assessed by Montgomery method[2, 3] (Extended Data Figure 7 and 7b). The analysis was carried out by using a van der Pauw geometry to calculate the conductivity anisotropy ρa/ρc\rho_a/\rho_c using (lw)2⋅Bα,k2\left(\frac{l}{w}\right)^2 \cdot B_{\alpha,k}^2, where ll and ww are sample dimensions and Bα,kB_{\alpha,k} is the conformal mapping function related to the ratio of van der Pauw resistance along different directions (Raa/RccR_{aa}/R_{cc}). The extracted anisotropy value is close to 4 at room temperature.

Hall measurements were performed in a PPMS (Quantum Design) equipped with a 14 T magnet. AC current was generated by a lock-in amplifier and passed through the device, VxxV_{xx}, VxyV_{xy} as well as the current IACI_{\mathrm{AC}} were recorded simultaneously. Carrier concentration nn and mobility μ\mu were extracted assuming a single carrier model. Extended Data Fig. 8 shows supplemental data from magneto-transport measurement. Unlike many other metallic CDW systems such as 2HNbSe2\mathrm{NbSe}_2 [4] and 1T-TiSe21T\text{-}\mathrm{TiSe}_2 [5], no carrier type switching behavior was observed across either of the two phase transitions, indicated by the plot of Hall voltage VxyV_{xy} vs. BB throughout the whole temperature range.

Single crystal X-ray diffraction

Single crystal diffraction at 130 K, 220 K and 298 K were carried out on beamline 12.2.1 at the Advanced Light Source (ALS), Lawrence Berkeley National Laboratory. Crystals were mounted on Mi-TeGen Kapton loops (Dual Thickness MicroMountsTM) and placed in a nitrogen cold stream on the goniometer head of a Bruker D8 diffractometer, equipped with a PHOTONII CPAD detector operating in shutter-less mode. Diffraction data were collected using monochromatic synchrotron radiation with a wavelength of 0.72880 Å using silicon (111) monochromator. A combination of ff and ω\omega scans with scan speeds of 1 s per 2 degrees for the ff scans, and 1 s per 0.15 degree for the ω\omega scans at 2θ=02\theta= 0 and -20°, respectively. The precession map was generated by Bruker APEX 3 with resolution 1.5 Å and thickness 0.1 with the refined unit cell. Note that the refined space group is different from previously reported P63mc1P6_3mc^1. It is mainly attributed to the improved brightness and resolution using synchrotron radiation that allows the observation of weak reflections. Detailed crystallography data and refinement results at different temperatures are listed in Extended Data Table 5 – Table 11.

Raman spectroscopy and Raman mode analysis

Polarization-resolved Raman spectroscopy was performed in a backscattering geometry using a confocal microscope spectrometer (Horiba Evolution). The incident beam (532 nm) was focused on a spot of size of 1–2 μm1\text{--}2\,\mu\mathrm{m} by using a 50 X objective lens. Laser power was set to 2.0 mW. The integration time of the spectrometer was 5 min. The beam was linearly polarized, and a half-wave plate was placed before the objective for polarization rotation. The analyzer was placed in front of the spectrometer entrance and was set parallel/perpendicular to the incident polarization when measuring XX or XY channel respectively. For polarization dependence scans, the half-wave plate was rotated from 0∘0^\circ to 180∘180^\circ with a 5∘5^\circ step.

Based on temperature dependent XRD data, we assume the following space and point groups at different temperatures. BaTiS3_3 undergoes two structural phase transitions in the temperature range from 4 K up to room temperature. From ∼250\sim250 K (Transition II) to 300 K, a hexagonal structure with space group: P63cmP6_3cm and point group: C6vC_{6v} (6mm6mm). From ∼160\sim160 K (Transition I) to ∼250\sim250 K, trigonal structure with space group: P3c1P3c1 and point group: C3vC_{3v} (3m3m). Below ∼160\sim160 K (Transition I), a monoclinic structure with space group: P21P2_1 and point group: C2C_2 (2).

Normal modes of the lattice form irreducible representations of the point group, therefore providing information about their Raman activity and symmetries in real space. The optical representations of the point groups above are as follows:

C6v (6mm): ΓRaman−active=8A1+15E1+15E2 (acoustic modes are not included)C_{6v}\ (6mm):\ \Gamma_{\mathrm{Raman-active}} = 8A_1 + 15E_1 + 15E_2\ \text{(acoustic modes are not included)}
C3v (3m): ΓRaman−active=59A1+119E (acoustic modes are not included)C_{3v}\ (3m):\ \Gamma_{\mathrm{Raman-active}} = 59A_1 + 119E\ \text{(acoustic modes are not included)}
C2 (2): ΓRaman−active=59A+58B (acoustic modes are not included)C_2\ (2):\ \Gamma_{\mathrm{Raman-active}} = 59A + 58B\ \text{(acoustic modes are not included)}

The peak intensity of a Raman scattering from a given mode QiQ_i is given by:

Ii∝∣e^s∂α~i∂Qie^i∣2(1)I_i \propto\left|\hat{e}_s \frac{\partial\tilde{\alpha}_i}{\partial Q_i} \hat{e}_i\right|^2 \tag*{(1)}

where α~i\tilde{\alpha}_i is a polarizability tensor element, and ∂α~i∂Qi\frac{\partial\tilde{\alpha}_i}{\partial Q_i} is a Raman tensor element for the mode QiQ_i.

e^s\hat{e}_s and e^i\hat{e}_i are polarization states of scattered and incident lights, respectively.

Analysis of Raman modes at room temperature (T=300T = 300 K)

We first consider room temperature hexagonal crystal structure with P63cmP6_{3}cm space group and C6vC_{6v} (6mm6mm) point group. The Raman tensors are given by:

A1=(a000a000b),E1=(00c000c00) and (00000c0c0),E2=(d000−d0000) and (0−d0−d00000)(2)A_{1} = \begin{pmatrix} a & 0 & 0 \\ 0 & a & 0 \\ 0 & 0 & b \end{pmatrix}, \quad E_{1} = \begin{pmatrix} 0 & 0 & c \\ 0 & 0 & 0 \\ c & 0 & 0 \end{pmatrix} \text{ and } \begin{pmatrix} 0 & 0 & 0 \\ 0 & 0 & c \\ 0 & c & 0 \end{pmatrix}, \qquad E_{2} = \begin{pmatrix} d & 0 & 0 \\ 0 & -d & 0 \\ 0 & 0 & 0 \end{pmatrix} \text{ and } \begin{pmatrix} 0 & -d & 0 \\ -d & 0 & 0 \\ 0 & 0 & 0 \end{pmatrix} \tag*{(2)}

We worked in a backscattering geometry on a (010) surface of BaTiS3_3. The incident light is along -yy direction and the reflected light is along +yy direction. In the parallel-polarization channel, we set e^s=e^i=(cos⁡θ,0,sin⁡θ)\hat{e}_{s} = \hat{e}_{i} = (\cos\theta, 0, \sin\theta), where θ\theta is an angle from x-axis. In the cross-polarization channel e^i=(cos⁡θ,0,sin⁡θ)\hat{e}_{i} = (\cos\theta, 0, \sin\theta) and e^s=(−sin⁡θ,0,cos⁡θ)\hat{e}_{s} = (-\sin\theta, 0, \cos\theta). From these we obtain polarization angle dependence of Raman peak intensities:

I(A1)∝∣e^sA1e^i∣2=[a(cos⁡θ)2+b(sin⁡θ)2]2(Parallel)(3)I(A_{1}) \propto\lvert\hat{e}_{s}A_{1}\hat{e}_{i}\rvert^{2} = [a(\cos\theta)^{2} + b(\sin\theta)^{2}]^{2} \quad(Parallel) \tag*{(3)}
I(A1)∝∣e^sA1e^i∣2=(a−b)2(sin⁡2θ)24(Cross)(4)I(A_{1}) \propto\lvert\hat{e}_{s}A_{1}\hat{e}_{i}\rvert^{2} = (a-b)^{2}\frac{(\sin2\theta)^{2}}{4} \quad(Cross) \tag*{(4)}

From polarization dependence of 385 cm−1^{-1} peak, we assign it to A1A_{1} mode.

The second Raman tensor matrix of E1E_{1} will be silent in both channels of (010) surface. The intensity of the first matrix is given by:

I(E1)∝∣e^sE1e^i∣2=c2(sin⁡2θ)2(Parallel)(5)I(E_{1}) \propto\lvert\hat{e}_{s}E_{1}\hat{e}_{i}\rvert^{2} = c^{2}(\sin2\theta)^{2} \quad(Parallel) \tag*{(5)}
I(E1)∝∣e^sE1e^i∣2=c2((cos⁡θ)2−(sin⁡θ)2)2(Cross)(6)I(E_{1}) \propto\lvert\hat{e}_{s}E_{1}\hat{e}_{i}\rvert^{2} = c^{2}((\cos\theta)^{2} - (\sin\theta)^{2})^{2} \quad(Cross) \tag*{(6)}

The sum of intensities in two channels of E1E_{1} is constant, independent of polarization angle.

Thus, we assign 187 cm−1^{-1} mode to E1E_{1} mode.

Since E2E_{2} modes are degenerate we add the intensities of two tensors.

I(E2)∝∣e^sE2e^i∣2=d2(cos⁡θ)4(Parallel)(7)I(E_{2}) \propto\lvert\hat{e}_{s}E_{2}\hat{e}_{i}\rvert^{2} = d^{2}(\cos\theta)^{4} \quad(Parallel) \tag*{(7)}
I(E2)∝∣e^sE2e^i∣2=d2(sin⁡2θ)24(Cross)(8)I(E_2) \propto|\hat{e}_s E_2 \hat{e}_i|^2 = \frac{d^2(\sin2\theta)^2}{4} \quad(Cross) \tag*{(8)}

We assigned 90 cm−1\mathrm{cm}^{-1} and 183 cm−1\mathrm{cm}^{-1} modes to E2E_2 symmetry. The results of room temperature mode analysis are summarized in Extended Data Table 1.

No.Frequency (cm−1\mathrm{cm}^{-1})Mode symmetry
190E2E_{2}
2183E2E_{2}
3185E1E_{1}
4385A1A_{1}

Table 1. List of room temperature Raman modes (T = 300 K).

Analysis of modes at low temperature (T = 15 K)

Next, we consider low temperature monoclinic structure of BaTiS3\mathrm{BaTiS}_3 at T = 15 K. The assumed group is P21P2_1 and the point group is C2C_2 (2). The Raman tensor for this point group is given by:

A=(ad0db000c),B=(00e00fef0)(9)A = \begin{pmatrix} a & d & 0 \\ d & b & 0 \\ 0 & 0 & c \end{pmatrix}, \qquad B = \begin{pmatrix} 0 & 0 & e \\ 0 & 0 & f \\ e & f & 0 \end{pmatrix} \tag*{(9)}

We worked in the backscattering geometry; thus, the Raman peak intensities are given by:

I(A)∝∣e^sAe^i∣2=[a(cos⁡θ)2+c(sin⁡θ)2]2(Parallel)(10)I(A) \propto|\hat{e}_s A\hat{e}_i|^2 = [a(\cos\theta)^2 + c(\sin\theta)^2]^2 \quad(Parallel) \tag*{(10)}
I(A)∝∣e^sAe^i∣2=(a−c)2(sin⁡2θ)24(Cross)(11)I(A) \propto|\hat{e}_s A\hat{e}_i|^2 = (a-c)^2 \frac{(\sin2\theta)^2}{4} \quad(Cross) \tag*{(11)}

The modes that assigned to AA symmetry, are labeled in the table below (Extended Data Table 2).

I(B)∝∣e^sBe^i∣2=e2(sin⁡2θ)2(Parallel)(12)I(B) \propto|\hat{e}_s B\hat{e}_i|^2 = e^2(\sin2\theta)^2 \quad(Parallel) \tag*{(12)}
I(B)∝∣e^sBe^i∣2=e2((cos⁡θ)2−(sin⁡θ)2)2(Cross)(13)I(B) \propto|\hat{e}_s B\hat{e}_i|^2 = e^2((\cos\theta)^2 - (\sin\theta)^2)^2 \quad(Cross) \tag*{(13)}

The sum of Raman peak intensities in the parallel and cross channels of B mode, should be polarization independent. So, we sum the intensities of the two channels and assign polarization independent modes to B modes. Another way of distinguishing the A and B modes is as follows: 1) A mode in parallel channel must be two-fold, while the B mode must be four-fold. 2) in cross channel, both A and B must be four-fold, but with opposite phases. The results of these analysis are provided in the Extended Data Table 2. We observe 13 A modes and 11 B modes.

No.Frequency (cm−1\mathrm{cm}^{-1})Mode symmetry
135A
256.5A
368.5B
476A
591A
6106.5A
7120.5B
8145A
9177A
10179B
11196A
12214B
13217B
14219A
15224.5A
16253A
17266.5B
18280.5B
19293A
20309B
21363B
22385A
23410B
24450B

Table 2. List of low temperature Raman modes (T = 15 K).

In Extended Data Figure 10 and 10e, we plot polarization dependent Raman spectra in cross (XY) and in parallel (XX) channels respectively, at 15 K. Symmetry assignments of the modes are done by fitting each mode with expected polarization dependencies, from the Raman tensors of the assumed space and point groups. The soft mode (35 cm−135\ \mathrm{cm}^{-1}) polarization angle dependence closely follows 385 cm−1385\ \mathrm{cm}^{-1} with A symmetry (Extended Data Figure 10). Extended Data Figure 10 shows temperature dependent Raman spectra in cross (XY) channel.

Extended Data Fig. 10: Temperature dependent Raman spectra and polarization dependence

Extended Data Figure 10. a, Temperature dependent Raman spectra in cross channel. Like parallel channel, new modes emerge below Transition I. b, Polar plot of polarization dependence of soft mode and the A1g_{1g} mode. The symmetry of soft mode in both channels coincides with the symmetry of A1g_{1g} mode. c, Polarization dependence of cross channel Raman spectrum, taken at 15 K. d, Polarization dependence of parallel channel Raman spectrum, taken at 15 K.

Transient reflectivity measurement

Experiments were performed with a Ti:sapphire oscillator lasing at the center wavelength of 760 nm (1.63 eV) and pulse duration of 25 fs was used. The repetition rate of the laser is 1.6 MHz and no cumulative heating effect was observed. The output was split into pump (higher intensity) and probe (low intensity) arms, with a translation stage placed on the probe path to induce time-delay between the two arms. To increase the signal to noise ratio of our setup, we modulate the pump intensity at 100 kHz. For faster data acquisition and averaging, the pump-probe delay is rapidly scanned at a rate of 5 Hz with an oscillating mirror. The reflected probe beam was sent directly to a photodiode. The signal from the photodiode is sent to a lock-in amplifier locked to the pump modulation frequency.

Tempearture dependent transient reflectivity measurements were performed from 80 K to 330 K. Signal traces at each temperature consist of incoherent electronic decay signal and coherent phonon oscillations (Fig. 3d). We fit the decay background with a single exponential function:

S(t)=Ae−tτ+B(14)S(t) = A e^{-\frac{t}{\tau}} + B \tag*{(14)}

where τ\tau is a decay rate. The temperature dependence of the decay rate exhibits a critical slowing down behavior, thus indicating an electronic phase transition in BaTiS3_3 near 240 K.

DFT calculations

The band structure of BaTiS3_3 in the three different phases were computed using DFT. The initial structures were taken from the refined crystal structures from XRD at different temperatures, which are assigned to have a space group of P63cmP6_3cm (298 K), P3c1P3c1 (220 K), and P21P2_1 (130 K), respectively. The structures were fully optimized by DFT. These calculations were done using the Vienna Ab initio Simulation Package (VASP)[6] with projector augmented wave (PAW) potentials[7].

The exchange-correlation energy was treated with the generalized gradient approximation (GGA) using the Perdew-Burke-Ernzerhof (PEB) functional[8]. A cutoff energy of 650 eV was used for the expansion of the plane waves. The convergence criteria were set to 10−810^{-8} eV for total energy and 10−410^{-4} eV/Å for atomic forces, respectively. The Brillouin zone was sampled using a Γ\Gamma-centered Monkhorst-Pack kk-points mesh[9], with maximum spacing of 0.05 Å−1^{-1} for structural relaxations and 0.02 Å−1^{-1} for static calculations, respectively.

For the calculation of the rsr_s parameter, density functional perturbation theory calculations[10] were performed to obtain the static dielectric constant (ε\varepsilon) with the same energy cutoff and kk-point sampling as the DFT calculations. The input parameters for rsr_s, such as the band effective mass (mb∗m_b^*), experimental carrier concentration (nn), and static dielectric constant (ε\varepsilon), are provided in the Extended Data Table 3.

Different morphologies of CVT-grown BaTiS₃ crystals

Figure Extended Data Fig. 1. Different morphologies of CVT-grown BaTiS₃ crystals. Optical images of a, thin BTS needle, b, thick BTS needle and c, BTS platelet. For ‘needle’-like samples, c-axis follows the direction of long edges and is easy to determine. Edges of terraces on BTS plates are useful in assigning the crystal orientations, which can be further confirmed by polarization-dependent Raman spectroscopy.

STM / STS study of BaTiS3 at room temperature

Figure 2 (PDF p. 29). Extended Data Fig. 2 | STM / STS study of BaTiS3_3 at room temperature. a, Surface morphology of freshly cleaved BaTiS3_3 crystal. b, Typical dI/dV\mathrm{d}I/\mathrm{d}V spectra on a freshly cleaved BaTiS3_3 crystal surface taken at room temperature. A small bandgap of ∼0.3 eV\sim0.3\ \mathrm{eV} was extracted from the spectra, consistent with the value measured from optical absorption spectra.

BaTiS3 bulk device fabrication with panels a, b and c

Figure 3 (PDF p. 30). BaTiS3_{3} bulk device fabrication. a, A cross-sectional illustration of a BaTiS3_{3} device for transport studies. Low-stressed polyimide is used for crystal embedding to minimize the extrinsic strain effect from thermal contraction. b, Optical microscopic images of BaTiS3_{3} devices with various electrode designs. c, Optical images of BaTiS3_{3} devices used for transport measurements.

Hall measurements

Figure 8. a, Plot of Hall voltage VxyV_{xy} with magnetic field from -6 T to 6 T at different temperatures. Hall data was collected from the Sample C, with its temperature-dependent longitudinal resistance illustrated in Extended Data Figure 4. b-c, The measured data (blue) were fitted linearly to extract the carrier concentration nn and mobility μ\mu.

Contour plot of transient reflectivity as a function of temperature and delay time

Extended Data Figure 11. Contour plot of transient reflectivity as a function of temperature and delay time. The transient reflectivity traces at different temperatures shown in Fig. 3c are cut and taken from this plot.

Space groupnn (cm−3^{-3})mbm_bεs\varepsilon_srsr_s
P21P2_11.69×10141.69 \times10^{14} (90 K)0.52259.6418.56
P3c1P3c18.18×10168.18 \times10^{16} (200 K)0.68241.584.43
P63cmP6_3cm8.99×10178.99 \times10^{17} (280 K)0.53935.161.86

Table 3. Input parameters used to compute the rsr_s value for BaTiS3_3.

BaTiS3_3 PlateletBaTiS3_3 Thin NeedleBaTiS3_3 Thick Needle
Space groupP63cmP6_3cmP63cmP6_3cmP63cmP6_3cm
Cell dimensions
aa, bb, cc (Å)11.671(2), 11.671(2), 5.833(2)11.686(2), 11.686(2), 5.840(2)11.670(2), 11.670(2), 5.846(2)
α\alpha, β\beta, γ\gamma (°)90.00(3), 90.00(3), 120.00(3)90.00(3), 90.00(3), 120.00(3)90.00(3), 120.00(3), 90.00(3)
Volume (Å3^3)688.1(3)690.7(3)689.4(3)
Density (g/cm3^3)4.0754.0604.067
Refinement
R1R_1, wR2wR_2 [all data]0.0308, 0.07690.0341, 0.07620.0366, 0.0606
R1R_1, wR2wR_2 [I>4σII > 4\sigma_I]0.0272, 0.07340.0326, 0.07470.0236, 0.0559
GoFGoF1.1261.1431.045
Merohedral Twinning−1 0 0 0 −1 0 0 0 −1 2−1 0 0 0 −1 0 0 0 −1 2−1 0 0 0 −1 0 0 0 −1 2
BASF0.530470.395200.39818

Table 4. Data collection and refinement statistics for various BaTiS3_3 morphologies at 300 K

BaTiS3_3 300KBaTiS3_3 220KBaTiS3_3 130K
Space groupP63cmP6_3cmP3c1P3c1P21P2_1
Cell dimensions
aa, bb, cc (Å)11.671(2), 11.671(2), 5.833(2)23.285(5), 23.285(5), 5.836(2)13.431(3), 5.817(2), 13.431(3)
α\alpha, β\beta, γ\gamma (°)90.00(3), 90.00(3), 120.00(3)90.00(3), 90.00(3), 120.00(3)90.00(3), 120.00(3), 90.00(3)
Volume (Å3^3)688.1(3)2740.0(15)908.8(5)
Density (g/cm3^3)4.0754.0934.114
Intensity Statistics
Resolution (Å)Inf. - 0.620.72 - 0.62Inf. - 0.620.72 - 0.62Inf. - 0.600.70 - 0.60
Completeness (%)99.9100.0100.0100.099.9100.0
Redundancy31.3018.3934.8919.0128.2817.41
Mean II / σI\sigma I34.1818.1322.4210.2732.4217.86
Reflections
RσR_{\sigma}, RintR_{\mathrm{int}}0.0170, 0.04980.0315, 0.06910.0479, 0.0499
θmin⁡\theta_{\min}, θfull\theta_{\mathrm{full}}, θmax⁡\theta_{\max} (°)2.015, 25.242, 34.7031.035, 25.930, 35.401.751, 25.242, 36.160
Friedel fraction full0.9900.9990.999
Refinement
Resolution (Å)∼ (Inf. - 0.62)∼ (Inf. - 0.62)50.0 - 0.60
No. reflections104679838676
No. I>2σII > 2\sigma I91666217161
No. parameters30185187
No. constraints111
R1R_1, wR2wR_2 [all data]0.0308, 0.07690.0420, 0.06920.0448, 0.0814
R1R_1, wR2wR_2 [I>4σII > 4\sigma I]0.0272, 0.07340.0305, 0.06570.0321, 0.0764
GoF1.1261.0580.969
Twinning-1 0 0 0 -1 0 0 0 -1 2-1 0 0 0 -1 0 0 0 1 -41 0 1 0 1 0 -1 0 0 -6
BASF0.530470.39520, 0.09971, 0.101310.21467, 0.10736, 0.19557, 0.19508, 0.12829
XNDP∼∼0.001

Table 5. Data collection and refinement statistics of BaTiS3_3 platelet at different temperatures

Atomx/ax/ay/by/bz/cz/cUisoU_{\mathrm{iso}} (A˚2\mathrm{\AA}^{2})OccupancySymmetry Order
Ba010.66577(3)00.2569(5)0.01861(15)12
Ti012/31/30.0668(4)0.0284(5)13
Ti02100.9287(3)0.0201(4)16
S0010.83416(10)00.7075(4)0.0147(4)12
S0020.83207(7)0.33219(7)0.2919(3)0.0161(3)11

Table 6. Atomic coordinates and equivalent isotropic atomic displacement parameters for 300K BaTiS₃.

AtomU11U_{11} (A˚2\mathrm{\AA}^{2})U22U_{22} (A˚2\mathrm{\AA}^{2})U33U_{33} (A˚2\mathrm{\AA}^{2})U23U_{23} (A˚2\mathrm{\AA}^{2})U13U_{13} (A˚2\mathrm{\AA}^{2})U12U_{12} (A˚2\mathrm{\AA}^{2})
Ba010.01549(17)0.0145(2)0.0255(2)0-0.00555(6)0.00723(10)
Ti010.0289(4)0.0289(4)0.0275(13)000.0145(2)
Ti020.0263(4)0.0263(4)0.0078(7)000.0131(2)
S0010.0124(4)0.0188(5)0.0151(9)00.0012(6)0.0094(3)
S0020.0113(4)0.0172(4)0.0218(9)-0.0013(4)-0.0014(5)0.0085(3)

Table 7. Anisotropic atomic displacement parameters for 300K BaTiS₃.

Atomx/ax/ay/by/bz/cz/cUisoU_{\mathrm{iso}} (Å2^2)OccupancySymmetry Order
Ba010.50086(5)0.16598(6)0.1488(4)0.0160(4)11
Ba020.33230(8)0.33184(3)0.12095(9)0.01285(14)11
Ba030.16619(5)0.16711(6)0.6390(2)0.0136(3)11
Ba040.33424(9)0.50007(5)0.67561(6)0.01412(17)11
Ti01000.4711(7)0.0151(7)13
Ti020.17477(12)0.33363(13)1.3939(8)0.0172(6)11
Ti032/31/3-0.0228(9)0.0200(10)13
Ti040.49169(13)0.49143(12)0.3953(6)0.0141(5)11
Ti051/32/30.5072(5)0.0164(4)13
Ti060.33335(16)0.17228(9)0.8064(3)0.0138(2)11
S0010.41913(17)0.41791(19)0.6766(8)0.0120(7)11
S0020.0823(2)0.3343(3)1.1338(10)0.0162(10)11
S0030.1654(3)0.2502(2)1.1191(10)0.0131(8)11
S0040.2481(2)0.4155(2)1.1245(12)0.0184(12)11
S0050.2502(2)0.0849(2)0.5836(8)0.0091(10)11
S0060.4158(2)0.1670(3)0.5860(9)0.0094(9)11
S0070.3337(3)0.25135(17)0.5774(4)0.0099(3)11
S0080.4980(3)0.4150(2)0.1661(7)0.0126(7)11
S0090.3321(3)0.58292(15)0.2306(5)0.0120(5)11
S0100.5826(2)0.2504(2)-0.2985(10)0.0106(7)11
S0110.08327(19)0.0824(2)0.1900(7)0.0105(6)11
S0120.4159(2)0.4996(3)0.1585(11)0.0131(9)11

Table 8. Atomic coordinates and equivalent isotropic atomic displacement parameters for 220K BaTiS3.

AtomU11U_{11} (A˚2\mathrm{\AA}^{2})U22U_{22} (A˚2\mathrm{\AA}^{2})U33U_{33} (A˚2\mathrm{\AA}^{2})U23U_{23} (A˚2\mathrm{\AA}^{2})U13U_{13} (A˚2\mathrm{\AA}^{2})U12U_{12} (A˚2\mathrm{\AA}^{2})
Ba010.0121(5)0.0106(4)0.0253(11)0.0010(4)0.0058(5)0.0057(4)
Ba020.0118(2)0.0108(4)0.0157(3)0.0038(3)0.0007(6)0.0054(3)
Ba030.0122(4)0.0120(4)0.0169(8)-0.0035(4)-0.0060(4)0.0064(3)
Ba040.0114(2)0.0128(4)0.0185(4)0.0048(4)0.0013(6)0.0063(4)
Ti010.0218(9)0.0218(9)0.0018(16)000.0109(5)
Ti020.0139(14)0.0241(12)0.0137(15)-0.0008(12)-0.0015(10)0.0096(12)
Ti030.0217(12)0.0217(12)0.017(2)000.0109(6)
Ti040.0157(15)0.0103(14)0.0109(13)0.0001(9)-0.0012(9)0.0026(7)
Ti050.0207(6)0.0207(6)0.0077(8)000.0103(3)
Ti060.0174(5)0.0154(10)0.0093(5)0.0002(7)-0.0002(12)0.0087(10)
S0010.0081(11)0.0068(11)0.0198(19)0.0035(11)0.0019(11)0.0027(8)
S0020.0144(13)0.0173(15)0.023(2)-0.0005(14)0.0018(14)0.0122(12)
S0030.0104(14)0.0085(12)0.0203(19)-0.0019(12)-0.0009(11)0.0046(10)
S0040.0069(13)0.0110(15)0.035(3)0.0029(16)0.0046(14)0.0031(12)
S0050.0075(16)0.0050(15)0.012(2)-0.0018(13)-0.0011(11)0.0011(14)
S0060.0098(17)0.0177(19)0.0014(16)-0.0003(14)-0.0017(10)0.0074(13)
S0070.0144(7)0.0123(14)0.0075(7)-0.0011(10)-0.0036(17)0.0101(13)
S0080.0143(13)0.0068(11)0.0158(18)-0.0003(11)0.0004(13)0.0046(9)
S0090.0130(8)0.0052(13)0.0161(11)0.0005(12)0.001(2)0.0032(13)
S0100.0110(16)0.0099(16)0.0081(15)-0.0001(12)0.0010(14)0.0031(11)
S0110.0081(16)0.0085(16)0.0123(14)-0.0009(14)0.0024(15)0.0023(10)
S0120.0103(14)0.0119(15)0.020(2)-0.0021(12)-0.0030(11)0.0076(11)

Table 9. Anisotropic atomic displacement parameters for 220K BaTiS3_3.

Atomx/ax/ay/by/bz/cz/cUisoU_{\mathrm{iso}} (Ų)OccupancySymmetry Order
Ba010.16964(18)0.0966(5)0.83377(19)0.0092(4)11
Ba020.33529(19)0.6180(3)0.66598(17)0.0083(3)11
Ba030.16408(19)0.1159(5)0.33356(17)0.0104(4)11
Ba040.33066(18)0.5974(5)0.16634(19)0.0097(4)11
Ti010.4834(5)-0.0783(11)0.4967(5)0.0071(8)11
Ti020.0157(5)0.4179(12)0.5016(5)0.0141(10)11
Ti030.5138(5)0.2949(12)0.9973(6)0.0096(9)11
Ti04-0.0137(5)0.7926(11)0.0019(6)0.0105(10)11
S0010.4196(6)0.073(2)0.8349(6)0.0128(16)11
S0020.0835(7)0.6528(18)0.4145(6)0.0079(17)11
S003-0.0847(6)0.1486(19)0.3346(6)0.0094(17)11
S0040.1644(6)0.137(2)0.5826(7)0.0091(14)11
S0050.4166(6)0.1589(18)0.5858(6)0.0078(13)11
S0060.6651(6)0.141(2)0.5824(7)0.0084(15)11
S0070.4151(6)0.1534(17)0.3342(5)0.0068(16)11
S0080.4175(6)0.086(2)1.0830(6)0.0143(17)11
S0090.3310(6)0.5666(19)0.9144(7)0.0132(18)11
S010-0.1689(6)0.5543(12)-0.0855(6)0.0059(11)11
S0110.0808(6)0.5578(13)0.1663(5)0.0060(11)11
S012-0.0817(6)1.0685(14)0.0824(6)0.0071(11)11

Table 10. Atomic coordinates and equivalent isotropic atomic displacement parameters for 130K BaTiS₃.

AtomU11U_{11} (A˚2\mathring{\mathrm{A}}^2)U22U_{22} (A˚2\mathring{\mathrm{A}}^2)U33U_{33} (A˚2\mathring{\mathrm{A}}^2)U23U_{23} (A˚2\mathring{\mathrm{A}}^2)U13U_{13} (A˚2\mathring{\mathrm{A}}^2)U12U_{12} (A˚2\mathring{\mathrm{A}}^2)
Ba010.0076(8)0.0124(11)0.0049(5)-0.0028(7)0.0011(5)-0.0013(6)
Ba020.0088(7)0.0082(8)0.0086(7)-0.0033(7)0.0048(5)-0.0013(7)
Ba030.0083(7)0.0158(10)0.0054(7)0.0021(7)0.0023(5)0.0004(7)
Ba040.0094(7)0.0121(11)0.0089(6)0.0024(7)0.0055(5)0.0018(6)
Ti010.011(2)0.0016(14)0.0109(17)0.0018(16)0.0071(17)0.0024(17)
Ti020.008(2)0.021(2)0.0116(18)-0.001(2)0.0040(17)-0.001(2)
Ti030.009(2)0.010(2)0.0118(19)0.0005(18)0.0061(16)-0.0017(19)
Ti040.013(2)0.009(2)0.0103(18)0.0030(17)0.0063(16)-0.0028(18)
S0010.008(3)0.023(4)0.006(3)-0.001(3)0.002(2)-0.002(3)
S0020.011(3)0.005(4)0.008(3)0.001(2)0.005(2)0.001(2)
S0030.008(3)0.009(4)0.010(3)0.000(2)0.004(2)-0.001(2)
S0040.007(3)0.013(4)0.004(2)0.000(2)-0.0001(19)0.001(2)
S0050.011(3)0.007(3)0.008(3)0.000(2)0.007(2)0.001(2)
S0060.007(3)0.010(4)0.010(2)0.000(3)0.005(2)-0.001(2)
S0070.009(3)0.008(4)0.002(2)-0.0008(19)0.002(2)0.000(2)
S0080.009(3)0.031(4)0.006(3)0.002(3)0.006(2)0.002(2)
S0090.008(3)0.023(5)0.008(3)0.003(3)0.004(2)0.003(3)
S0100.006(2)0.002(2)0.007(2)-0.0017(17)0.0018(19)-0.0025(17)
S0110.011(3)0.002(2)0.005(2)-0.0009(17)0.0039(19)-0.0019(18)
S0120.010(3)0.001(2)0.010(2)-0.0014(17)0.0056(19)-0.0002(16)

Table 11. Anisotropic atomic displacement parameters for 130K BaTiS3\mathrm{BaTiS_3}.

References

  1. [1]Grüner, G. The dynamics of charge-density waves. Reviews of Modern Physics 60, 1129 (1988).
  2. [2]Johannes, M. & Mazin, I. Fermi surface nesting and the origin of charge density waves in metals. Physical Review B 77, 165135 (2008).
  3. [3]Zhu, X., Guo, J., Zhang, J. & Plummer, E. Misconceptions associated with the origin of charge density waves. Advances in Physics: X 2, 622-640 (2017).DOI
  4. [4]Rossnagel, K. On the origin of charge-density waves in select layered transition-metal dichalcogenides. Journal of Physics: Condensed Matter 23, 213001 (2011).DOI
  5. [5]Torchinsky, D. H., Mahmood, F., Bollinger, A. T., Božović, I. & Gedik, N. Fluctuating charge-density waves in a cuprate superconductor. Nature Materials 12, 387-391 (2013).
  6. [6]Gerber, S. et al. Three-dimensional charge density wave order in YBa₂Cu₃O₆.₆₇ at high magnetic fields. Science 350, 949-952 (2015).
  7. [7]Ishihara, S. & Nagaosa, N. Interplay of electron-phonon interaction and electron correlation in high-temperature superconductivity. Physical Review B 69, 144520 (2004).DOI
  8. [8]Sipos, B. et al. From Mott state to superconductivity in 1T-TaS₂. Nature Materials 7, 960-965 (2008).DOI
  9. [9]Ma, L. et al. A metallic mosaic phase and the origin of Mott-insulating state in 1T-TaS₂. Nature Communications 7, 1-8 (2016).DOI
  10. [10]Neupert, T., Denner, M. M., Yin, J.-X., Thomale, R. & Hasan, M. Z. Charge order and superconductivity in kagome materials. Nature Physics, 1-7 (2021).
  11. [14]Peierls, R. & Peierls, R. E. Quantum Theory of Solids. (Oxford University Press, 1955).
  12. [15]Thorne, R. E. Charge-density-wave conductors. Physics Today 49, 42-47 (1996).
  13. [16]Achkar, A. et al. Orbital symmetry of charge-density-wave order in La₁.₈₇₅Ba₀.₁₂₅CuO₄ and YBa₂Cu₃O₆. ⁶⁷. Nature Materials 15, 616-620 (2016).
  14. [17]Frano, A. et al. Long-range charge-density-wave proximity effect at cuprate/manganate interfaces. Nature Materials 15, 831-834 (2016).DOI
  15. [18]Cercellier, H. et al. Evidence for an Excitonic Insulator Phase in 1T–TiSe₂. Physical Review Letters 99, 146403 (2007).
  16. [19]Kidd, T., Miller, T., Chou, M. & Chiang, T.-C. Electron-hole coupling and the charge density wave transition in TiSe₂. Physical Review Letters 88, 226402 (2002).
  17. [20]Lu, Y. et al. Zero-gap semiconductor to excitonic insulator transition in Ta₂NiSe₅. Nature Communications 8, 1-7 (2017).DOI
  18. [21]Nakano, A. et al. Antiferroelectric distortion with anomalous phonon softening in the excitonic insulator Ta₂NiSe₅. Physical Review B 98, 045139 (2018).DOI
  19. [22]Lv, B. et al. Unconventional hysteretic transition in a charge density wave. Physical Review Letters 128, 036401 (2022).
  20. [23]Wu, D. et al. Layered semiconductor EuTe₄ with charge density wave order in square tellurium sheets. Physical Review Materials 3, 024002 (2019).DOI
  21. [24]Di Salvo, F. J., Moncton, D. & Waszczak, J. Electronic properties and superlattice formation in the semimetal TiSe₂. Physical Review B 14, 4321 (1976).DOI
  22. [25]Kitou, S. et al. Effect of Cu intercalation and pressure on excitonic interaction in 1T–TiSe₂. Physical Review B 99, 104109 (2019).DOI
  23. [26]Rossnagel, K., Kipp, L. & Skibowski, M. Charge-density-wave phase transition in 1T–TiSe₂: Excitonic insulator versus band-type Jahn-Teller mechanism. Physical Review B 65, 235101 (2002).DOI
  24. [27]Niu, S. et al. Giant optical anisotropy in a quasi-one-dimensional crystal. Nature Photonics 12, 392-396 (2018).
  25. [28]Sun, B. et al. High frequency atomic tunneling yields ultralow and glass-like thermal conductivity in chalcogenide single crystals. Nature Communications 11, 1-9 (2020).DOI
  26. [29]Tsutsumi, K. et al. Direct electron-diffraction evidence of charge-density-wave formation in NbSe₃. Physical Review Letters 39, 1675 (1977).DOI
  27. [30]Moncton, D., Axe, J. & DiSalvo, F. Study of superlattice formation in 2H-NbSe₂ and 2H-TaSe₂ by neutron scattering. Physical Review Letters 34, 734 (1975).
  28. [31]Hodeau, J. et al. Charge-density waves in NbSe₃ at 145K: Crystal structures, X-ray and electron diffraction studies. Journal of Physics C: Solid State Physics 11, 4117 (1978).DOI
  29. [32]Inami, T. et al. Symmetry breaking in the metal-insulator transition of BaVS₃. Physical Review B 66, 073108 (2002).
  30. [33]Zhang, K. et al. Raman signatures of inversion symmetry breaking and structural phase transition in type-II Weyl semimetal MoTe₂. Nature Communications 7, 1-6 (2016).DOI
  31. [34]Xi, X. et al. Strongly enhanced charge-density-wave order in monolayer NbSe₂. Nature Nanotechnology 10, 765-769 (2015).DOI
  32. [35]Goli, P., Khan, J., Wickramaratne, D., Lake, R. K. & Balandin, A. A. Charge density waves in exfoliated films of van der Waals materials: evolution of Raman spectrum in TiSe₂. Nano Letters 12, 5941-5945 (2012).DOI
  33. [36]Gadermaier, C. et al. Electron-phonon coupling in high-temperature cuprate superconductors determined from electron relaxation rates. Physical Review Letters 105, 257001 (2010).
  34. [37]Demsar, J., Biljaković, K. & Mihailovic, D. Single particle and collective excitations in the one-dimensional charge density wave solid K₀.₃MoO₃ probed in real time by femtosecond spectroscopy. Physical Review Letters 83, 800 (1999).DOI
  35. [38]Lin, T. et al. Optical spectroscopy and ultrafast pump-probe study on Bi₂Rh₃Se₂: Evidence for charge density wave order formation. Physical Review B 101, 205112 (2020).DOI
  36. [39]Nakamura, M. et al. Metal-semiconductor transition and Luttinger-liquid behavior in quasi-one-dimensional BaVS₃ studied by photoemission spectroscopy. Physical Review B 49, 16191 (1994).
  37. [40]Wada, T., Shimada, M. & Koizumi, M. Synthesis of Ba(V₁−ₓTiₓ)S₃ (0 ≤ x ≤ 1.0) compounds and their structural transitions. Journal of Solid State Chemistry 33, 357-359 (1980).DOI
  38. [41]Kim, S.-J. et al. Structure and physical properties of the barium niobium sulfides BaNbS₃ and BaNb₀.₈S₂.₈. Journal of Solid State Chemistry 115, 427-434 (1995).
  39. [42]Montgomery, H. Method for measuring electrical resistivity of anisotropic materials. Journal of applied physics 42, 2971-2975 (1971).
  40. [43]Borup, K. A., Fischer, K. F., Brown, D. R., Snyder, G. J. & Iversen, B. B. Measuring anisotropic resistivity of single crystals using the van der Pauw technique. Physical Review B 92, 045210 (2015).DOI
  41. [44]Ong, N. P. & Brill, J. Conductivity anisotropy and transverse magnetoresistance of NbSe₃. Physical Review B 18, 5265 (1978).DOI
  42. [45]Smontara, A., Tkalčec, I., Bilušić, A., Budimir, M. & Berger, H. Anisotropy of the thermal conductivity in (TaSe₄)₂I. Physica B: Condensed Matter 316, 279-282 (2002).
  43. [46]Ceperley, D. M. & Alder, B. J. Ground state of the electron gas by a stochastic method. Physical Review Letters 45, 566 (1980).
  44. [47]Rastelli, G. & Ciuchi, S. Wigner crystallization in a polarizable medium. Physical Review B 71, 184303 (2005).
  45. [48]Fratini, S. & Quémerais, P. Polarization catastrophe in the polaronic Wigner crystal. The European Physical Journal B-Condensed Matter and Complex Systems 29, 41-49 (2002).DOI

Paper details

vlnc:W_nf5qzjge
Version
v1 · latest
Published
Fresh — added to the Hub within the last 30 days
Added
License
CC BY 4.0
Usage

views · 0

downloads · 0

A view counts once per browser per day, a download each time the PDF is requested.

  • Physics and Astronomy

Not recorded for this paper

View statement
Looking for related papers…
Contents