Giant Anomalous Hall Conductivity and Gilbert Damping in Room-temperature Ferromagnetic Half-Heusler Alloys PtMnBi

Abstract

Half-Heusler alloys have emerged as promising candidates for novel spintronic applications due to their exceptional properties including the high Curie temperature (TC) above room temperature and large anomalous Hall conductivity (AHC). In this work, we systematically study the magnetic and electronic properties of PtMnBi in α-, {beta}-, and γ-phase using first-principles calculations and Monte Carlo simulations. The three phases are found to be ferromagnetic metals. In particular, the α-phase PtMnBi shows a high TC up to 802 K and a relatively large Gilbert damping of 0.085. Additionally, the γ-phase PtMnBi possesses a non-negligible AHC, reaching 203 Ω-1cm-1 at the Fermi level. To evaluate its potential in nanoscale devices, we further investigate the α-phase PtMnBi thin films. The Gilbert dampings of α-phase PtMnBi thin films varies with film thickness and we attribute this variation to the distinct band structures at the high-symmetry point Γ, which arise from differences in film thickness. Moreover, the 1-layer (1L) α-phase thin film retains robust ferromagnetism (TC = 688 K) and shows enhanced Gilbert damping (0.14) and AHC (1116 Ω-1cm-1) compared to the bulk. Intriguingly, under a 2% in-plane biaxial compressive strain, the Gilbert damping of 1L α-phase PtMnBi thin film increases to 0.17 and the AHC reaches 2386 Ω-1cm-1. The coexistence of giant Gilbert damping and large AHC makes α-phase PtMnBi a compelling platform for practical spintronic applications, and highlights the potential of half-Heusler alloys in spintronic device design.

*Corresponding authors: [email protected]

Introduction

The limitations of conventional electronic devices have driven the research focus toward the spintronics that harness both spin and charge degrees of freedom simultaneously for information processing [1]. Among diverse magnetic materials that hold promise for advancing the spintronics, the Heusler alloys including both full-Heusler and half-Heusler alloys have emerged as a captivating research focal point. The first Heusler alloy Cu2MnAl\mathrm{Cu}_{2}\mathrm{MnAl} discovered by Heusler exhibits ferromagnetism, despite that its constituent elements themselves are non-magnetic [2, 3]. This unique feature sparked significant interest in exploring the potentials of Heusler alloys further. Moreover, the properties of Heusler alloys can be finely engineered by tuning their elemental composition [4, 5]. Given the vast number of possible elemental combinations, Heusler alloys can realize a rich and diverse array of properties, such as superconductivity [6, 7, 8, 9], half-metallic ferromagnetism [10, 11, 12, 13], and high Curie temperature [14, 15]. These remarkable properties render them promising candidates for practical applications in the next generation of spintronic devices.

The temporal evolution of the magnetization M\mathbf{M} in a ferromagnetic (FM) material is captured by the Landau-Lifshitz-Gilbert equation [16, 17, 18]

dMdt=−γM×Heff+αMSM×dMdt(1)\frac{d\mathbf{M}}{dt}=-\gamma\mathbf{M}\times\mathbf{H}_{\mathrm{eff}}+\frac{\alpha}{M_{\mathrm{S}}}\mathbf{M}\times\frac{d\mathbf{M}}{dt} \tag*{(1)}

The right of the Landau-Lifshitz-Gilbert equation is composed of two terms, namely, the precession term (i.e., the first term) and the damping term (i.e., the second term). The precession term captures the rotational motion of the magnetization M\mathbf{M} around the effective magnetic field, Heff\mathbf{H}_{\mathrm{eff}}, while the damping term accounts for the gradual decay of this precession[18]. The dimensionless parameter α\alpha in Eq. (1) is the Gilbert damping parameter, which characterizes the rate of energy dissipation during the precession of the magnetization M\mathbf{M}. The performance of a wide range of spintronic devices, including hard disk drives, magnetic random-access memories and magnetic sensors, is governed by the Gilbert damping α\alpha[19].

To date, only low Gilbert damping parameters are found in Heusler alloys. Among them, Co2\mathrm{Co}_{2}-based full-Heusler alloys, such as Co2MnSi\mathrm{Co}_{2}\mathrm{MnSi}, Co2MnAl\mathrm{Co}_{2}\mathrm{MnAl}, and Co2MnGe\mathrm{Co}_{2}\mathrm{MnGe}, have been confirmed to exhibit ultra-low Gilbert dampings, in the order of 10−410^{-4} [20, 21, 22]. Recently, experimental measurements have revealed that the Gilbert damping of the half-Heusler alloy NiMnSb thin film reaches an order of magnitude of 10−310^{-3} [23, 24]. This implies that Mn-based half-Heusler alloys may have a relatively higher Gilbert damping. On the other hand, the synergy between spin-orbit coupling (SOC) and time-reversal symmetry breaking could engender a fascinating transport phenomenon termed the anomalous Hall effect (AHE)[25], which has been extensively investigated[26, 27]. Singh et al. [28] have successfully measured the AHC of PtMnSb (with a TCT_{\mathrm{C}} of 560 K) which is as high as 2.2×1032.2 \times10^{3} Ω−1\Omega^{-1}cm−1^{-1} at 2 K. Due to the heavier atomic mass and stronger SOC of Bi compared to Sb, the SOC in PtMnBi is enhanced, implying the potential for a larger AHC. So, it is of importance to perform a systematic investigation into the Gilbert dampings and AHE in PtMnBi.

In this work, the magnetic and electronic properties of α\alpha-, β\beta-, and γ\gamma-phase PtMnBi are systematically investigated using first-principles calculations. Our results indicate that the TCT_{\mathrm{C}} of α\alpha-phase PtMnBi reaches 802 K, which is significantly higher than room temperature. Among the three phases, γ\gamma-phase PtMnBi displays the highest AHC at the Fermi level, achieving a remarkable value of 203 Ω−1\Omega^{-1}cm−1^{-1}. Notably, each phase of PtMnBi exhibits a large AHC exceeding 1000 Ω−1\Omega^{-1}cm−1^{-1} when the Fermi level is shifted to about 2 eV, suggesting that the huge AHC of PtMnBi can be realized experimentally by doping electrons. Besides, the α\alpha-phase PtMnBi exhibits a relatively large Gilbert damping, in the order of 10−210^{-2}. We find that the Gilbert damping varies with the thickness of PtMnBi thin films, which is attributed to the modulation of the band structure at the high-symmetry point Γ\Gamma by the film thickness. Remarkably, 1-layer (1L) PtMnBi thin film shows an impressively high TCT_{\mathrm{C}} of 688 K, a giant AHC (1116 Ω−1\Omega^{-1}cm−1^{-1}) and a large Gilbert damping (α=0.14\alpha= 0.14). Intriguingly, when a 2% biaxial compressive strain is applied to 1L α\alpha-phase PtMnBi, its spin polarization is enhanced to 70.62%. Meanwhile, the AHC at the Fermi level reaches an extraordinarily large value of 2386 Ω−1\Omega^{-1}cm−1^{-1}, and the Gilbert damping attains a big value up to 0.17. The coexistence of high spin polarization, substantial AHC, and giant Gilbert damping in 1L PtMnBi thin film endows it with remarkable potential for applications. Our findings demonstrate the promising potential of half-Heusler alloy PtMnBi for versatile applications in spintronic devices.

Computational methods

The density functional theory (DFT) calculations are conducted using the Vienna ab initio simulation package (VASP) [29]. Projector-augmented wave pseudopotentials are utilized to describe the interactions between core and valence electrons [30, 31]. We treat Mn-3d4s, Pt-5d6s and Bi-6s6p as valence electrons. For the depiction of exchange-correlation interactions, we employ the generalized gradient approximation formulated by Perdew, Burke and Ernzerhof [32]. We adopt an energy cutoff of 400 eV and a kk-mesh grid of 21×21×2121 \times21 \times21 centered at the Γ\Gamma point. The three phases of PtMnBi are fully relaxed until the forces on each atom are less than 0.01 eV/Å. The energy convergence criterion is 10−610^{-6} eV. Based on magnetic interaction parameters derived from DFT calculations, the TCT_{\mathrm{C}}s are obtained through Monte Carlo simulations.

Within the framework of scattering theory, the Gilbert damping parameters can be ascertained by first-principles calculations via the linear response formalism [33, 34, 35]. The reliability of this approach has been verified in previous studies [36, 37, 38]. By extending the torque method initially developed for studying magnetic anisotropy energy [39, 40], the Gilbert damping can be calculated by employing the following formula [41]:

αμν=−πℏγMs∑ij⟨ψi∣∂H∂uμ∣ψj⟩⟨ψj∣∂H∂uν∣ψi⟩×δ(EF−Ei)δ(EF−Ej)(2)\alpha_{\mu\nu}=-\frac{\pi\hbar\gamma}{M_s}\sum_{ij}\left\langle\psi_i\left|\frac{\partial H}{\partial u_\mu}\right|\psi_j\right\rangle\left\langle\psi_j\left|\frac{\partial H}{\partial u_\nu}\right|\psi_i\right\rangle\times\delta(E_F-E_i)\delta(E_F-E_j) \tag*{(2)}

In Eq. (2), MsM_s, γ\gamma and EFE_F represent saturation magnetization, gyromagnetic ratio and the Fermi level, respectively. uμu_\mu is the deviation of a normalized magnetic moment away from its equilibrium. In Eq. (2), the delta function δ(EF−E)\delta(E_F-E) is replaced by the Lorentzian function L(E)=0.5Γ/[π(E−E0)2+π(0.5Γ)2]L(E)=0.5\Gamma/[\pi(E-E_0)^2+\pi(0.5\Gamma)^2] with the scattering rate Γ\Gamma characterizing the temperature effect. To facilitate the calculations, we employ unit cells of three phases of PtMnBi to compute their Gilbert dampings, and simultaneously increase the kk-point mesh to 31×31×3131 \times31 \times31 to ensure the numerical convergence. When calculating the Gilbert dampings of α\alpha-phase PtMnBi thin films, a kk-point mesh of 47×47×147 \times47 \times1 is used.

Results and Discussion

The half-Heusler alloy with a 1:1:1 stoichiometric ratio and general formula XYZ crystallizes in the face-centered cubic C1b\mathrm{C1b} crystal structure (space group F-43m, No. 216). The C1b\mathrm{C1b} crystal structure is constructed from three interpenetrating face-centered cubic sublattices. Constituting atoms occupy the Wyckoff positions 4a (0, 0, 0), 4b (1/2, 1/2, 1/2) and 4c (1/4, 1/4, 1/4), with the 4a-4b and 4a-4c atomic pairs forming NaCl-type and ZnS-type sublattices, respectively. Due to the presence of three nonequivalent element arrangements within this crystal structure, the half-Heusler alloy exhibits three distinct phases, namely, the α\alpha-, β\beta- and γ\gamma-phase. For PtMnBi alloy, X and Y represent the transition metals Pt and Mn, respectively, and Z denotes the main group element Bi. Figure 1(a)-(Figure 1f) illustrate the crystal structures of the α\alpha-, β\beta- and γ\gamma-phase, in which Pt-Mn-Bi occupy the Wyckoff positions 4c-4b-4a, 4a-4b-4c and 4b-4c-4a, respectively.

Image not extracted

Figure 1. Top and side views of crystal structures of (a) (d) α\alpha-phase, (b) (e) β\beta-phase and (c) (f) γ\gamma-phase PtMnBi. (g) The first three nearest-neighbor Heisenberg exchange paths are shown by green arrows. (h) The first Brillouin zone of PtMnBi.

Structural optimizations are performed using the unit cells of α\alpha-, β\beta- and γ\gamma-phase PtMnBi. Their corresponding optimized lattice constants are 6.406, 6.465, and 6.310 Å, with their primitive cell energies of -19.412, -18.005 and -18.725 eV, respectively. It is evident that α\alpha-phase PtMnBi has the lowest energy, while γ\gamma-phase has the smallest lattice constant. These results are in good agreement with previous theoretical studies[42]. After determining the structural characteristics of the three phases of PtMnBi, we explore their magnetic properties. Among the three phases of PtMnBi, γ\gamma-phase exhibits the smallest magnetic moment (3.471 μB\mu_B/Mn), compared to 3.959 μB\mu_B/Mn in the α\alpha-phase and 3.949 μB\mu_B/Mn in the β\beta-phase. These different magnetic moments can be qualitatively interpreted based on the structural configurations of the neighbor atoms. In the γ\gamma-phase, Mn atoms with Pt and Bi atoms as their nearest neighbors and possessing the lowest electronegativity among them, lose most of their electrons, thus giving rise to the smallest magnetic moment [43].

To determine the magnetic ground state of PtMnBi, a spin Hamiltonian composed of the first three nearest-neighbor (NN) Heisenberg exchange interactions is adopted. The spin Hamiltonian takes the following form:

H=∑ijJijSi⋅Sj(3)H = \sum_{ij} J_{ij}\mathbf{S}_i \cdot\mathbf{S}_j \tag*{(3)}

In Eq. (3), Si\mathbf{S}_i and Sj\mathbf{S}_j correspond to the spin at magnetic sites ii and jj, respectively, and JijJ_{ij} defines the coupling parameter mediating the Heisenberg exchange interaction between spins Si\mathbf{S}_i and Sj\mathbf{S}_j. Note that a negative JijJ_{ij} denotes a FM Heisenberg exchange coupling, and a positive JijJ_{ij} denotes an antiferromagnetic (AFM) one. We employ the energy mapping based on first-principles calculations to estimate Heisenberg exchange interaction parameters[44]. Table S1 and Fig. S1 in the supplementary material (SM) provide the constructed magnetic configurations and the magnetic moments of each Mn atom in α\alpha-phase PtMnBi, respectively. As illustrated in Figure 2(a), our calculations reveal that the Heisenberg exchange parameters for all three phases of PtMnBi are negative, indicating that all of them could exhibit a FM ground state. Explicitly, the calculated J1J_1 for the α\alpha-, β\beta- and γ\gamma-phase PtMnBi are -11.461, -0.037, and -0.497 meV, respectively. The corresponding J2J_2 are -5.276, -5.219, and -4.114 meV, and the J3J_3 are -2.753, -1.676, and -0.515 meV. We can see that the values of J1J_1, J2J_2 and J3J_3 of α\alpha-phase PtMnBi are the largest among the three phases, indicating that it possesses the strongest FM Heisenberg coupling interactions. In different phases, the variation of J1J_1 is remarkably pronounced, and the changes in J2J_2 and J3J_3 remain relatively minor. To determine the magnetic anisotropy, we calculate the energies of α\alpha-, β\beta- and γ\gamma-phase PtMnBi with their magnetizations being along the [100], [11] and [111] directions, respectively. As shown in Figure 2(b), the results suggest that the magnetic easy axes of α\alpha-, β\beta- and γ\gamma-phase are [100], [11] and [111], respectively.

Image not extracted

Figure 2. Magnetic properties of PtMnBi. (a) Heisenberg exchange parameters JJ. (b) DFT calculated energies when the magnetization directions are along [100], [11], and [111]. For each phase, the lowest energy is set as the reference. (c) TCT_\mathrm{C}s obtained by Monte Carlo simulations. (d) The Γ\Gamma-dependent Gilbert dampings.

Within the mean field approximation, the TCT_\mathrm{C} of a ferromagnet can be estimated using the following relationship [44]:

TC=S(S+1)3kB∑lzlJl(4)T_\mathrm{C} = \frac{S(S+1)}{3k_\mathrm{B}} \sum_l z_l J_l \tag*{(4)}

In Eq. (4), the summation is run over all the near neighbors of a given spin site, with ziz_i representing the coordination number of adjacent neighbors connected by JiJ_i. Based on Eq. (4), we see that the TCT_\mathrm{C} exhibits a direct proportionality to ziz_i and the strength of the Heisenberg exchange interaction JiJ_i. Using Eq. (4), the TCT_\mathrm{C}s of PtMnBi in α\alpha-, β\beta- and γ\gamma-phase are calculated to be 1389, 418, and 250 K, respectively. Given that the mean field approximation tends to overestimate magnetic transition temperatures [45], we also employ Monte Carlo simulations to determine the TCT_\mathrm{C} of PtMnBi. Excitingly, our results indicate that the TCT_\mathrm{C} of α\alpha-phase PtMnBi is as high as 802 K [Fig. 2(c)]. The TCT_\mathrm{C}s of β\beta- and γ\gamma-phase PtMnBi are 254 and 163 K, respectively. The high TCT_\mathrm{C}, especially above the room temperature, is crucial for their potential applications in practical spintronic devices.

Figure 2(d) depicts the Γ\Gamma-dependent Gilbert dampings of α\alpha-phase PtMnBi. We see that its Gilbert damping exhibits a characteristic behavior: it initially decreases and subsequently increases as the scattering rate Γ\Gamma rises. This trend is in accordance with previous studies [19, 41, 46, 47]. Within the framework of the breathing Fermi surface model, the Gilbert damping is composed of both intraband and interband contributions. As the scattering rate Γ\Gamma increases, the interband contribution increases whereas the intraband contribution decreases, thereby resulting in a non-monotonic dependence of the Gilbert damping on the scattering rate [48]. Considering the practical applications of half-Heusler alloy PtMnBi, we focus on discussing its Gilbert damping at Γ=26\Gamma= 26 meV, which corresponds to room temperature. At room temperature, the α\alpha-phase PtMnBi exhibiting a Gilbert damping parameter of 0.085, which is much larger than the Gilbert damping of body-centered cubic (bcc) Fe (α=0.0013\alpha= 0.0013) [19]. The higher Gilbert damping α\alpha is, the more rapidly energy is dissipated, allowing the magnetization to reach equilibrium more quickly [49]. This rapid relaxation behavior is of vital importance to magnetic storage technologies.

Now, we investigate the electronic structures of different phases of PtMnBi. The electronic band structures of α\alpha-, β\beta- and γ\gamma-phase PtMnBi are calculated along the high-symmetry paths X-W-L-Γ\Gamma-X-K-U-Γ\Gamma. Figures S2(a), (c) and (e) in the SM show their band structures when SOC is not included in our DFT calculations. These band structures indicate that three phases of PtMnBi are metallic. The projected density of states (PDOS) for the three phases given in Figs. S2 (b), (d) and (f) reveal that the electronic states near the Fermi level in all three phases of PtMnBi are predominantly contributed by Mn and Pt atoms. Considering the strong SOC of Bi atoms, we study the electronic band structures of PtMnBi with SOC [Figs. 3(a), 3(c) and 3(e)]. As shown in Figure 3(b), Figure 3(d) and Figure 3(f), the PDOSs with SOC are similar to those without SOC. For α\alpha-phase PtMnBi, we see that SOC induces significant changes in the band structure near the Fermi level at the high-symmetry Γ\Gamma point, characterized by the opening of a bandgap at crossing bands [Fig. 3 (a)]. By contrast, the β\beta- and γ\gamma-phase PtMnBi exhibit relatively minor changes in their bands near the Fermi level at the Γ\Gamma point under the influence of SOC.

Image not extracted

Figure 3. Electronic properties and AHC of PtMnBi. (a) Band structures and (b) PDOS of the α\alpha-phase with SOC being considered. (c) and (d) are same as (a) and (b) but for the β\beta-phase. (e) and (f) are same as (a) and (b) but for the γ\gamma-phase. (g) The dependence of AHC on the Fermi level position for the three phases of PtMnBi.

In ferromagnets where time-reversal symmetry is broken, the presence of strong SOC may give rise to AHE. To explore the AHE in PtMnBi, we construct an effective tight binding model via employing Wannier90 package [50]. The projected orbitals of Pt-s, pp, dd, Mn-s, pp, dd, and Bi-s, pp are used here. Figures S3(a)-Figure 2(c) demonstrate the close consistency between Wannier-interpolated band structures and DFT results. As shown in Figure 3(g), the evolution of AHC with the Fermi level is calculated by WannierTools package [51] when the magnetizations of the three phases are aligned along their easy axes. It is noteworthy that the AHC of γ\gamma-phase PtMnBi reaches a large value of 203 Ω−1cm−1\Omega^{-1}\mathrm{cm}^{-1} at the Fermi level. In contrast, the α\alpha- and β\beta-phase PtMnBi exhibit significantly lower AHC, with values of 17 and 45 Ω−1cm−1\Omega^{-1}\mathrm{cm}^{-1}, respectively. Besides, within a range of 1.5 eV around the Fermi level, there are some very large values of AHC. Especially, at 1.43 eV above the Fermi level, the AHC of α\alpha-phase PtMnBi reaches a value of 1278 Ω−1cm−1\Omega^{-1}\mathrm{cm}^{-1}. For β\beta-phase PtMnBi, AHC reaches a value of 686 Ω−1cm−1\Omega^{-1}\mathrm{cm}^{-1} when the Fermi level is located at 0.40 eV. When the Fermi level is shifted to -1.48 eV, the AHC of γ\gamma-phase PtMnBi can reach a huge value of 1394 Ω−1cm−1\Omega^{-1}\mathrm{cm}^{-1}. These results suggest that the Fermi level can be tuned by doping electrons or holes to achieve larger AHC in experiments.

For practical applications, device miniaturization is becoming increasingly important. In recent years, thin films of the half-Heusler alloy NiMnSb have been successfully fabricated[52]. Inspired by this, studying the electronic structures and the Gilbert dampings of PtMnBi thin films is also of importance. Our interest is dedicated to α\alpha-phase PtMnBi, which stands out for its highest TCT_{\mathrm{C}} (802 K) and maximum Gilbert damping (0.085). Here, we construct different slab models with varying numbers of layers—specifically, 1L, 2-layer (2L), 3-layer (3L), 4-layer (4L), and 5-layer (5L)—to simulate thin films of α\alpha-phase PtMnBi. Each model is equipped with a vacuum space of 15 Å to prevent spurious interactions, and their structural configurations are shown in Fig. 4(a) (depicting only the 1L and 2L systems) and Fig. S4(a) (depicting the 3L, 4L and 5L systems). Based on Eq. (3), we first investigate the magnetic properties of 1L α\alpha-phase PtMnBi thin film. The calculated exchange parameters J1J_1, J2J_2, and J3J_3 are -14.335, -9.780 and -30.243 meV, respectively, indicating FM couplings for all three interactions. Our Monte Carlo simulations confirm a FM ground state with a TCT_{\mathrm{C}} of 688 K. Meanwhile, we calculate its magnetic anisotropy energy and find that its magnetic easy axis is out-of-plane (i.e., zz axis). Considering the typical suppression of TCT_{\mathrm{C}} with reduced thickness, the TCT_{\mathrm{C}}s of α\alpha-phase PtMnBi thin films should still remain above room temperature [53].

Image not extracted

Figure 4.

Image not extracted

Figure 4 (PDF p. 10). Side views of crystal structures of (a) 1L and 2L α\alpha-phase PtMnBi thin films. (b) Thickness-dependent Gilbert dampings in α\alpha-phase PtMnBi films at Γ=26\Gamma= 26 meV. (c) The band structure with SOC considered and (e) kk-dependent contributions to the Gilbert damping of 1L α\alpha-phase PtMnBi thin film at Γ=26\Gamma= 26 meV. (d) and (f) Same as (c) and (e) but for 2L α\alpha-phase PtMnBi thin film.

Given that α\alpha-phase PtMnBi thin films are room temperature ferromagnets, we next calculate their Gilbert dampings at the scattering rate Γ=26\Gamma= 26 meV and illustrate the result in Fig. 4(b). One can observe that the Gilbert damping of 1L α\alpha-phase PtMnBi thin film is remarkably large up to 0.14, which significantly exceeds its bulk counterpart (0.085). When the thickness of the thin film exceeds 2L, the variation in Gilbert dampings becomes negligible. It is worth noting that, compared to 1L α\alpha-phase PtMnBi thin film, the Gilbert damping of 2L α\alpha-phase PtMnBi thin film is reduced by 78.6 %. To gain a deeper understanding of the variations in Gilbert dampings, we examine band structures and kk-dependent contributions to Gilbert dampings in 1L and 2L α\alpha-phase PtMnBi thin films. As depicted in Figs. 4(c) and 4(d), compared with 1L α\alpha-phase PtMnBi thin film, the positions of bands crossing the Fermi level in 2L film undergo a significant shift. Especially, the bands at high-symmetry points, particularly those at the Γ\Gamma point, exhibit distinct differences. By examining the kk-dependent contributions to Gilbert damping [Figs. 4(e)-4(f)], we can see that the kk points that make significant contributions are predominantly located in the proximity of the Fermi level (marked by arrows). It should be noted that not all kk points with energies in the proximity of the Fermi level make significant contributions to Gilbert damping. Their contributions also depend on the matrix element ⟨ψi∣∂H∂uμ∣ψj⟩⟨ψj∣∂H∂uν∣ψi⟩\langle\psi_i \mid\frac{\partial H}{\partial u_\mu} \mid\psi_j \rangle\langle\psi_j \mid\frac{\partial H}{\partial u_\nu} \mid\psi_i \rangle. Moreover, in 1L α\alpha-phase PtMnBi thin film, the primary contributions to Gilbert damping originate from the vicinity of the high-symmetry Γ\Gamma point and X-M path, whereas in 2L α\alpha-phase PtMnBi thin film it primarily stems from the X-M path only. In other words, the Gilbert damping of 2L α\alpha-phase PtMnBi thin film has sharply decreased because the bands near the high-symmetry Γ\Gamma point have been tuned to a position far away from the Fermi level compared with those of 1L thin film. To gain an in-depth understanding of the mechanism for which the number of layers tunes the Gilbert damping, we also investigate the band structures and kk-dependent contributions to Gilbert dampings in 3L, 4L and 5L α\alpha-phase PtMnBi thin films. As shown in fig:S5 in the SM, the band structures near the high-symmetry Γ\Gamma point also undergo significant changes, which are the main reason for the reduced contributions to the Gilbert dampings. Overall, by varying the thickness of α\alpha-phase PtMnBi thin films, one can effectively tune the band structures near the high-symmetry Γ\Gamma point, thereby engineering the Gilbert damping.

During the experimental growth of half-Heusler alloy thin films, lattice mismatch induced by substrates can induce strain and changes in electronic band structures. Therefore, investigating the properties of α\alpha-phase PtMnBi thin films under in-plane biaxial strain is of significant importance for advancing their practical applications. Here, we focus specifically on the study of 1L α\alpha-phase PtMnBi thin film due to their remarkably large Gilbert damping.

The spin-polarized band structure and PDOS depicted in Figure 5(a) and Figure 5(b) demonstrate that 1L α\alpha-phase PtMnBi thin film exhibits metallic characteristics, with the electronic states near the Fermi level being primarily contributed by Pt, Mn, and Bi atoms. We observe that the bands crossing the Fermi level are predominantly provided by the majority spin states. In contrast, for the minority spin states, only the bands at the high-symmetry point Γ\Gamma intersect the Fermi level. The spin polarization (PP) can be calculated as follows [54],

Image not extracted

Figure 5. Electronic and magnetic properties of 1L α\alpha-phase PtMnBi thin film. (a) Spin-polarized band structure and (b) PDOS. (c) The relationship between in-plane biaxial compressive strain and spin polarization, PP. (d) The AHC values at the Fermi level under in-plane biaxial compressive strain when the magnetization direction is along the zz axis. (e) The impact of in-plane compressive strain on Gilbert damping at Γ=26\Gamma= 26 meV with the magnetization directions along the zz axis.

P=N↑−N↓N↑+N↓(5)P = \frac{N_{\uparrow} - N_{\downarrow}}{N_{\uparrow} + N_{\downarrow}} \tag*{(5)}

In Eq. (5), N↑N_{\uparrow} and N↓N_{\downarrow} denote the total density of states (DOS) for the majority and minority states at the Fermi level, respectively. We approximate PP by employing the integral total DOS within 23 meV near the Fermi level. Figure 5(c) depicts the correlation between the in-plane biaxial compressive strain and PP in 1L α\alpha-phase PtMnBi thin film. Overall, the spin polarization of the system rises as the applied strain increases. Notably, when the applied stress reaches 2% or higher, the spin polarization exceeds 70%. This value is remarkably higher than that of the α\alpha-, β\beta-, and γ\gamma-phase of bulk PtMnBi, which exhibit spin polarizations of 21.99%, 33.93%, and 33.23%, respectively. It is worth mentioning that when the lattice constant of α\alpha-phase PtMnBi is reduced from -3% to -11.2%, it will become a half-metal with 100% spin polarization[42].

To gain a comprehensive understanding of the AHE in 1L PtMnBi thin film, we calculate its AHC both before and after the application of biaxial compressive strain. As shown in Figure 5(d), the AHC of 1L α\alpha-phase PtMnBi thin film at the Fermi level reaches an impressive value of 1116 Ω−1cm−1\Omega^{-1}\mathrm{cm}^{-1}, surpassing the AHC of all bulk phases of PtMnBi as well as that of bcc Fe (751 Ω−1cm−1\Omega^{-1}\mathrm{cm}^{-1}) [55]. Moreover, the application of compressive strain to thin film results in an increase in its AHC at the Fermi level. Notably, when the in-plane biaxial compressive strain is 2% and 5%, the AHCs at the Fermi level reach giant values of 2386 and 2600 Ω−1cm−1\Omega^{-1}\mathrm{cm}^{-1}, respectively. Figure S6 illustrates the distribution of Berry curvature in the first Brillouin zone of 1L α\alpha-phase PtMnBi thin film. We find that, regardless of whether compressive strain is applied, significant Berry curvatures exist near the point Γ\Gamma, thus leading to the large AHC. In contrast, the application of tensile strain results in a reduction of the AHC at the Fermi level in 1L α\alpha-phase PtMnBi thin film (see Fig. S7(a) in the SM).

Figure 5(e) illustrates the strain-dependent variation in the Gilbert dampings of 1L α\alpha-phase PtMnBi thin film with out-of-plane magnetization orientation (i.e., M∥zM \parallel z axis). Our calculations reveal that the Gilbert damping of 1L α\alpha-phase PtMnBi thin film remains larger than that of its bulk counterpart and other thicknesses of PtMnBi thin films, even after the application of in-plane biaxial compressive strain. Meanwhile, the application of compressive strain has a negligible effect on the Gilbert damping of 1L α\alpha-phase PtMnBi thin film. Specifically, as the external strain varies, the Gilbert dampings oscillate between 0.17 and 0.09. These indicate that the significantly large Gilbert dampings can be still maintained, despite the presence of lattice mismatch during the experimental fabrication of PtMnBi thin films. Besides, compressive strain effectively modifies the band structures near the Γ\Gamma point in 1L system, thereby inducing changes in Gilbert damping. However, the large Gilbert damping originates from the contributions of all kk-points within the first Brillouin zone (see Figs S8 and S9 in the SM). It is worth noting that tensile strain reduces the Gilbert damping of 1L α\alpha-phase PtMnBi thin film (see Fig. S7(b) in the SM). A higher Gilbert damping allows the magnetization to achieve equilibrium more swiftly, which is of paramount importance to magnetic storage technologies. Therefore, the 1L α\alpha-phase PtMnBi thin film, which features high spin polarization, a large AHC, and a significant Gilbert damping, holds tremendous potential in the design of advanced spintronic devices.

Conclusion

In summary, we systematically investigate the magnetic and electronic properties of α\alpha-, β\beta-, and γ\gamma-phase PtMnBi through first-principles calculations and Monte Carlo simulations. Our results reveal that α\alpha-phase PtMnBi exhibits an exceptionally high TCT_{\mathrm{C}} of 802 K, with a room-temperature large Gilbert damping (0.085). We demonstrate that the band structures at the high-symmetry point Γ\Gamma of α\alpha-phase PtMnBi thin films can be modulated by changing the film thickness, thereby enabling the control of their Gilbert dampings. Notably, the 1L α\alpha-phase PtMnBi thin film exhibits a remarkably high TCT_{\mathrm{C}} of 688 K, accompanied by a huge AHC of 1116 Ω−1cm−1\Omega^{-1}\mathrm{cm}^{-1} and a giant Gilbert damping of 0.14. Interestingly, when a 2% in-plane biaxial compressive strain is applied, the spin polarization of 1L PtMnBi thin film reaches 70.62%, and the Gilbert damping is as high as 0.17. Moreover, the AHC (2386 Ω−1cm−1\Omega^{-1}\mathrm{cm}^{-1}) at the Fermi level is significantly enhanced. The coexistence of high spin polarization, large AHC and significant Gilbert damping in 1L PtMnBi thin film renders them highly promising for developing next-generation spintronic devices. Our work provides valuable theoretical guidance for the potential application of the half-Heusler alloy PtMnBi in spintronic devices.

Declarations The authors declare that they have no competing interests and there are no conflicts.

Acknowledgements This work was supported by the National Key Research Program of China (Grant No. 2024YFA1408303 and 2022YFA1403301), the National Natural Sciences Foundation of China (Grant No. 12474247 and 92165204). Yusheng Hou acknowledges support from Guangdong Provincial Key Laboratory of Magnetoelectric Physics and Devices (Grant No. 2022B1212010008) and Research Center for Magnetoelectric Physics of Guangdong Province (Grant No. 2024B0303390001). Density functional theory calculations are performed on Tianhe-Xingyi.

References

  1. [1]I. Žutić, J. Fabian, and S. D. Sarma, Spintronics: Fundamentals and applications, Rev. Mod. Phys. 76, 323 (2004).DOI
  2. [2]F. Heusler, W. Starck, and E. Haupt, Magnetisch-chemische studien, Verh. Dtsch. Phys. Ges 5, 219 (1903).
  3. [3]F. Heusler and V. Dtsch, Mangan-aluminium-kupferlegierungen, Verh. DPG 5, 219 (1903).
  4. [4]H. C. Kandpal, C. Felser, and R. Seshadri, Covalent bonding and the nature of band gaps in some half-Heusler compounds, J. Phys. D: Appl. Phys. 39, 776 (2006).DOI
  5. [5]D. Shrivastava, N. Acharya, and S. P. Sanyal, in AIP Conf. Proc. (AIP Publishing, 2018).
  6. [6]H. Xiao, T. Hu, W. Liu, Y. Zhu, P. Li, G. Mu, J. Su, K. Li, and Z. Mao, Superconductivity in the half-Heusler compound TbPdBi, Phys. Rev. B 97, 224511 (2018).DOI
  7. [7]N. P. Butch, P. Syers, K. Kirshenbaum, A. P. Hope, and J. Paglione, Superconductivity in the topological semimetal YPtBi, Phys. Rev. B Condens. Matter 84, 220504 (2011).DOI
  8. [8]T. Bay, T. Naka, Y. Huang, and A. De Visser, Superconductivity in noncentrosymmetric YPtBi under pressure, Phys. Rev. B Condens. Matter 86, 064515 (2012).DOI
  9. [9]M. Meinert, Unconventional superconductivity in YPtBi and related topological semimetals, Phys. Rev. Lett. 116, 137001 (2016).DOI
  10. [10]R. A. de Groot, F. M. Mueller, P. G. v. Engen, and K. H. J. Buschow, New Class of Materials: Half-Metallic Ferromagnets, Phys. Rev. Lett. 50, 2024 (1983).
  11. [11]R. A. de Groot and K. H. J. Buschow, Recent developments in half-metallic magnetism, J. Magn. Magn. Mater 54-57, 1377 (1986).
  12. [12]M. Jourdan et al., Direct observation of half-metallicity in the Heusler compound Co2MnSi, Nat. Commun. 5, 3974 (2014).DOI
  13. [13]H. C. Kandpal, G. H. Fecher, and C. Felser, Calculated electronic and magnetic properties of the half-metallic, transition metal based Heusler compounds, J. Phys. D: Appl. Phys. 40, 1507 (2007).DOI
  14. [14]S. Wurmehl, G. H. Fecher, H. C. Kandpal, V. Ksenofontov, C. Felser, and H.-J. Lin, Investigation of Co2FeSi: The Heusler compound with highest Curie temperature and magnetic moment, Appl. Phys. Lett. 88 (2006).DOI
  15. [15]M. Meinert, J.-M. Schmalhorst, and G. Reiss, Exchange interactions and Curie temperatures of Mn2CoZ compounds, J. Phys.: Condens. Matter 23, 116005 (2011).DOI
  16. [16]L. Landau and E. Lifshitz, On the theory of the dispersion of magnetic permeability in ferromagnetic bodies, Phys. Z. Sowjetunion 8, 101 (1935).
  17. [17]T. L. Gilbert, A Lagrangian Formulation of the Gyromagnetic Equation of the Magnetization Field, Physical Review D 100, 1243 (1955).
  18. [18]T. L. Gilbert, A phenomenological theory of damping in ferromagnetic materials, IEEE Trans. Magn. 40, 3443 (2004).DOI
  19. [19]K. Gilmore, Y. Idzerda, and M. D. Stiles, Identification of the Dominant Precession-Damping Mechanism in Fe, Co, and Ni<? format?> by First-Principles Calculations, Phys. Rev. Lett. 99, 027204 (2007).pubmed.ncbi.nlm.nih.gov/17678253
  20. [20]C. de Melo, C. Guillemard, A. M. Friedel, V. Palín, J. C. Rojas-Sánchez, S. Petit-Watelot, and S. Andrieu, Unveiling transport properties of Co2MnSi Heusler epitaxial thin films with ultra-low magnetic damping, Appl. Mater. Today 25, 101174 (2021).
  21. [21]C. Guillemard et al., Ultralow magnetic damping in Co 2 Mn-based Heusler compounds: Promising materials for spintronics, Phys. Rev. Appl. 11, 064009 (2019).
  22. [22]B. Pradines, R. Arras, I. Abdallah, N. Biziere, and L. Calmel(s), First-principles calculation of the effects of partial alloy disorder on the static and dynamic magnetic properties of Co 2 MnSi, Phys. Rev. B 95, 094425 (2017).
  23. [23]P. Dürrenfeld et al., Tunable damping, saturation magnetization, and exchange stiffness of half-Heusler NiMnSb thin films, Physical Review B 92, 214424 (2015).DOI
  24. [24]R. Mandal et al., Nanoscale-thick ni-based half-heusler alloys with structural ordering-dependent ultralow magnetic damping: implications for spintronic applications, ACS Appl. Nano Mater. 5, 569 (2022).DOI
  25. [25]N. Nagaosa, J. Sinova, S. Onoda, A. H. MacDonald, and N. P. Ong, Anomalous hall effect, Rev. Mod. Phys. 82, 1539 (2010).DOI
  26. [26]H. Zhang, W. Yang, Y. Ning, and X. Xu, Abundant valley-polarized states in two-dimensional ferromagnetic van der Waals heterostructures, Phys. Rev. B 101, 205404 (2020).DOI
  27. [27]H. Zhang, W. Yang, P. Cui, X. Xu, and Z. Zhang, Prediction of monolayered ferromagnetic ${\mathrm{CrMnI}}_{6}$ as an intrinsic high-temperature quantum anomalous Hall system, Phys. Rev. B 102, 115413 (2020).
  28. [28]S. Singh, A. García-Page, J. Noky, S. Roychowdhury, M. G. Vergniory, H. Borrmann, H. H. Klauss, C. Felser, and C. Shekhar, Extended Berry Curvature Tail in Ferromagnetic Weyl Semimetals NiMnSb and PtMnSb, Adv. Sci. 11, 2404495 (2024).DOI
  29. [29]G. Kresse and J. Furthmüller, Efficient iterative schemes for ab initio total-energy calculations using a plane-wave basis set, Phys. Rev. B 54, 11169 (1996).pubmed.ncbi.nlm.nih.gov/9984901
  30. [30]P. E. Blöchl, Projector augmented-wave method, Phys. Rev. B 50, 17953 (1994).pubmed.ncbi.nlm.nih.gov/9976227
  31. [31]G. Kresse and D. Joubert, From ultrasoft pseudopotentials to the projector augmented-wave method, Phys. Rev. B 59, 1758 (1999).DOI
  32. [32]J. P. Perdew, K. Burke, and M. Ernzerhof, Generalized gradient approximation made simple, Phys. Rev. Lett. 77, 3865 (1996).pubmed.ncbi.nlm.nih.gov/10062328
  33. [33]A. Brataas, Y. Tserkovnyak, and G. E. W. Bauer, Scattering Theory of Gilbert Damping, Phys. Rev. Lett. 101, 037207 (2008).arxiv.org/abs/0807.5009
  34. [34]A. Brataas, Y. Tserkovnyak, and G. E. W. Bauer, Magnetization dissipation in ferromagnets from scattering theory, Phys. Rev. B 84, 054416 (2011).DOI
  35. [35]S. Mankovsky, D. Ködderitzsch, G. Woltersdorf, and H. Ebert, First-principles calculation of the Gilbert damping parameter via the linear response formalism with application to magnetic transition metals and alloys, Phys. Rev. B 87, 014430 (2013).DOI
  36. [36]M. A. W. Schoen, D. Thonig, M. L. Schneider, T. J. Silva, H. T. Nembach, O. Eriksson, O. Karis, and J. M. Shaw, Ultra-low magnetic damping of a metallic ferromagnet, Nat. Phys. 12, 839 (2016).DOI
  37. [37]L. Chen et al., Emergence of anisotropic Gilbert damping in ultrathin Fe layers on GaAs(001), Nat. Phys. 14, 490 (2018).DOI
  38. [38]X. Yang et al., Anisotropic nonlocal damping in ferromagnet/α-GeTe bilayers enabled by splitting energy bands, Phys. Rev. Lett. 131, 186703 (2023).DOI
  39. [39]X. Wang, R. Wu, D.-s. Wang, and A. Freeman, Torque method for the theoretical determination of magnetocrystalline anisotropy, Phys. Rev. B 54, 61 (1996).pubmed.ncbi.nlm.nih.gov/9984224
  40. [40]J. Hu and R. Wu, Control of the Magnetism and Magnetic Anisotropy of a Single-Molecule Magnet<?> format?> with an Electric Field, Phys. Rev. Lett. 110, 097202 (2013).pubmed.ncbi.nlm.nih.gov/23496742
  41. [41]Y. Hou and R. Wu, Strongly enhanced Gilbert damping in 3 d transition-metal ferromagnet monolayers in contact with the topological insulator Bi 2 Se 3, Phys. Rev. Appl. 11, 054032 (2019).
  42. [42]W. Huang, X. Wang, X. Chen, W. Lu, L. Damewood, and C. Fong, Structural and electronic properties of half-Heusler alloys PtXBi (with X= Mn, Fe, Co and Ni) calculated from first principles, J. Magn. Magn. Mater. 377, 252 (2015).DOI
  43. [43]W. Huang, X. Wang, X. Chen, W. Lu, L. Damewood, and C. Y. Fong, Structural and electronic properties of half-Heusler alloy PdMnBi calculated from first principles, Mater. Chem. Phys. 148, 32 (2014).DOI
  44. [44]H. Xiang, C. Lee, H.-J. Koo, X. Gong, and M.-H. Whangbo, Magnetic properties and energy-mapping analysis, Dalton Trans. 42, 823 (2012).DOI
  45. [45]V. R. Pavizhakumari, T. Skovhus, and T. Olsen, Beyond the random phase approximation for calculating Curie temperatures in ferromagnets: application to Fe, Ni, Co and monolayer CrI3, J. Phys.: Condens. Matter 37, 115806 (2025).DOI
  46. [46]S.-B. Zhao, X.-F. Huang, Z.-q. Wang, R. Wu, and Y. Hou, Thickness-dependent anisotropic Gilbert damping in heterostructures of ferromagnets and two-dimensional ferroelectric bismuth monolayers, Phys. Rev. B 110, 094435 (2024).DOI
  47. [47]L. Qiu, Z. Wang, X.-S. Ni, D.-X. Yao, and Y. Hou, Electrically tunable Gilbert damping in van der Waals heterostructures of two-dimensional ferromagnetic metals and ferroelectrics, Appl. Phys. Lett. 122 (2023).DOI
  48. [48]K. Gilmore, M. Stiles, J. Seib, D. Steiauf, and M. Fähnle, Anisotropic damping of the magnetization dynamics in Ni, Co, and Fe, Phys. Rev. B Condens. Matter 81, 174414 (2010).
  49. [49]S. Azzawi, A. Hindmarch, and D. Atkinson, Magnetic damping phenomena in ferromagnetic thin-films and multilayers, J. Phys. D: Appl. Phys. 50, 473001 (2017).DOI
  50. [50]A. A. Mostofi, J. R. Yates, Y.-S. Lee, I. Souza, D. Vanderbilt, and N. Marzari, wannier90: A tool for obtaining maximally-localised Wannier functions, Comput. Phys. Commun. 178, 685 (2008).DOI
  51. [51]Q. Wu, S. Zhang, H.-F. Song, M. Troyer, and A. A. Soluyanov, WannierTools: An open-source software package for novel topological materials, Comput. Phys. Commun. 224, 405 (2018).
  52. [52]F. Gerhard, C. Schumacher, C. Gould, and L. Molen kamp, Control of the magnetic in-plane anisotropy in off-stoichiometric NiMnSb, J. Appl. Phys. 115 (2014).
  53. [53]R. Zhang and R. F. Willis, Thickness-Dependent Curie Temperatures of Ultrathin Magnetic Films: Effect of the Range of Spin-Spin Interactions, Phys. Rev. Lett. 86, 2665 (2001).pubmed.ncbi.nlm.nih.gov/11290006
  54. [54]I. I. Mazin, How to define and calculate the degree of spin polarization in ferromagnets, Phys. Rev. Lett. 83, 1427 (1999).DOI
  55. [55]Y. Yao, L. Kleinman, A. MacDonald, J. Sinova, T. Jungwirth, D.-s. Wang, E. Wang, and Q. Niu, First principles calculation of anomalous Hall conductivity in ferromagnetic bcc Fe, Phys. Rev. Lett. 92, 037204 (2004).pubmed.ncbi.nlm.nih.gov/14753904

Paper details

vlnc:W_pewpfexs
Version
v1 · latest
Published
Fresh — added to the Hub within the last 30 days
Added
License
CC BY 4.0
Usage

views · 6

downloads · 0

A view counts once per browser per day, a download each time the PDF is requested.

  • Physics and Astronomy

Not recorded for this paper

View statement
Looking for related papers…
Contents