betaFeedback

WorksPhysics and Astronomy

Local magnetic correlations and light-sensitive centers in the Cr2AlC MAX phase

Abstract

Cr2AlC MAX phase is synthesized by high-pressure solid-state annealing and investigated as a candidate platform for optically responsive magnetism. Structural characterization confirms the formation of the Cr2AlC phase, while magnetic and optical-magnetic properties are examined by superconducting quantum interference device (SQUID) magnetometry, electron spin resonance (ESR), and first principles calculations. SQUID magnetometry identifies Cr 2AlC as a weak, field-linear metallic paramagnet dominated by Pauli-like susceptibility of itinerant Cr-derived states. Its non-monotonic temperature dependence is described by an additional contribution from antiferromagnetically coupled Cr-Cr dimers, whereas the low-temperature Curie-like upturn originates from only a trace population of localized Cr centers. Under red-light illumination, SQUID magnetometry does not reveal an intrinsic macroscopic optomagnetic response. In contrast, ESR at 4 K shows a reversible light-induced reduction of a local magnetic signal, but the optically modified spin population corresponds only to several tens of ppm of the Cr sublattice. Ab initio Bethe-Salpeter equation (ai-BSE) calculations combined with the maximally localized Wannier function analysis suggest that optical excitation can redistribute spin polarization between neighboring Cr sites with the opposite local moments. The combined experiment-theory approach therefore establishes the hierarchy of magnetic contributions in Cr 2AlC and identifies the microscopic origin of its local optical sensitivity. This provides a reference for designing MAX phases and related MXenes in which defects, surface terminations or reduced dimensionality may enhance optically active magnetic states.

Introduction

Controlled manipulation of magnetization might be utilized to store information. The industry and society has a need to increase the density of information, speed up of the reading and writing processes, and improve energy efficiency. Optical manipulation of magnetism has important advantages over traditional application of magnetic fields and represents significant step towards this goal. This concept has a potential to form the technology for the construction of novel magnetoelectronic and optomagnetic devices acting not only as information storage, but also as spin current generators/injectors, sensors, transducers or spin transistors [1].

The discovery of optical manipulation of magnetization employing femtosecond lasers [2] attracted a lot of interest both from basic research and industry. It represented a source of novel information on magnetism and introduced a possibility to examine magnetic systems far from equilibrium [3]. Multiple microscopic mechanisms were proposed to explain how the interaction with photons in the optical range induced magnetization changes. These included electron-phonon scattering [4, 5, 6], electron-magnon scattering [7, 8], spin-dependent transport of excited electrons [9], the optically induced intersite spin transfer in multicomponent systems [10] and many others [11]. Notably, many of these mechanisms strongly relied on the spin-orbit coupling [12], while others did not require it. The mechanisms were supported by multiple arguments, and debates about their role did not yet lead to conclusions. It appeared that more of such mechanisms could be present simultaneously, and for different systems diverse effects and processes dominated [13]. Recent calculations demonstrated difficulties connected to the interpretation of physical observables in the case of strong coupling between electrons and light, and revealed the importance of electron correlations [14].

Particularly interesting problem was the magnetization manipulation in antiferromagnets (AFM) [15]. The presence of antiparallel aligned sublattices introduced a new quality into the problem of optically induced magnetization change since each of these sublattices could act as the source or sink of angular momentum for the other one [16]. On the other hand, an observation of magnetization dynamics in the AFMs was significantly more challenging problem than in the ferromagnetic (FM) systems due to the absence of total magnetization. Therefore, successful measurements of spin dynamics in the AFMs had been made only in the last few years. Evolution of sublattice magnetization had been measured in a Gd-based layered AFM employing the resonant x-ray diffraction (focused on peak connected to the AF order) and ARPES [17, 18]. It was also possible to study the dynamics of AFMs indirectly, by measuring the spin emission induced by the optical pump [19]. Optical pumping led to a change of the resistance in AFM CuMnAs that was associated with the magnetization reorientation [20]. Theoretical works focused on the possibility to rotate the magnetization direction in the AFM materials via a torque exerted by light [21], especially for the case with the circularly polarized light where the inverse Faraday effect took place [22].

MAX phases are ternary transition-metal-based carbides, nitrides and carbonitrides given by formula Mn+1_{n+1}AXn_n, where M represents an early transition metal, A is an A-group element (mostly groups IIIA and IVA), and X denotes carbon or nitrogen [23]. They are precursors to obtain MXenes, materials with great promise for multiple applications, including their use in flexible and wearable electronics [24, 25]. This materials platform is therefore relevant for attempts to combine robust layered conductors with magnetic or spintronic functionality [26, 27]. Notably, MXenes are also known for good stability at ambient conditions [25], as compared e.g. to transition metal trihalides exhibiting 2D magnetism [28]. Magnetic order had been predicted in many of MXene type compounds, in some cases persisting even up to room temperature [24, 25], but the related experimental data were scarce. First experimental evidence of magnetic ordering had been found in Cr2_2TiC2_2Tx_x [29] (Tx_x denoted stabilizing surface terminations). The possibility to manipulate magnetism had been demonstrated in Ti3_3C2_2Tx_x, which exhibited weak ferro- or antiferromagnetism that could be further tuned by doping [30]. Magnetism had also been sought in the MAX phases, and the presence and stability of magnetic order was found to strongly depend on sample quality [23].

In Cr2AlC\mathrm{Cr}_{2}\mathrm{AlC}, the indications of weak magnetism (originating from ab initio calculations and from x-ray magnetic circular dichroism) had been heavily debated [31], most works concluded that it was nonmagnetic without extra doping [32, 33]. Due to the above given reasons it is highly interesting to examine optical control of magnetism in a material from the MAX family, where this phenomenon has remained largely unexplored experimentally.

Here, we combine experiment and theory to assess the magnetic and optomagnetic response of the Cr2AlC\mathrm{Cr}_{2}\mathrm{AlC} MAX phase. We synthesize Cr2AlC\mathrm{Cr}_{2}\mathrm{AlC} and characterize its structure and composition by x-ray diffraction, electron microscopy and energy-dispersive x-ray spectroscopy. The magnetic response is examined by superconducting quantum interference device (SQUID) magnetometry and electron spin resonance (ESR), combining measurements in the dark and influenced by illumination. Magnetometry identifies Cr2AlC\mathrm{Cr}_{2}\mathrm{AlC} as a weak metallic paramagnet dominated by a Pauli-like susceptibility, with an additional non-monotonic contribution assigned to local antiferromagnetic Cr-Cr correlations and only a trace Curie-like term from dilute localized centers. No macroscopic light-induced magnetic response is detected by magnetometry under red-light illumination. In contrast, ESR reveals a reversible light-induced reduction of a local magnetic signal at 4 K, which corresponds to only a very small fraction of Cr sites. To interpret this local optical sensitivity, we perform ab initio calculations of the electronic structure and optical transitions solving the Bethe-Salpeter equation, combined with an analysis of the band character based on maximally localized Wannier functions. Our results establish the hierarchy of magnetic contributions in Cr2AlC\mathrm{Cr}_{2}\mathrm{AlC} and identify the local character of the optically sensitive response. This provides a useful reference point for future searches of optomagnetism in MAX phases and related MXene systems, where surface terminations, defects and reduced dimensionality may enhance magnetic states that remain only marginal in bulk Cr2AlC\mathrm{Cr}_{2}\mathrm{AlC}.

Materials and methods

Materials Growth

Cr2AlC\mathrm{Cr}_{2}\mathrm{AlC} has been obtained by a solid state reaction (SSR). The powders: chromium (100 mesh; 99.5 % Aldrich), aluminium (325 mesh; 99.5 % Alfa Acesar) and carbon (graphite, < 20 μ\mum Aldrich) have been mixed in a Cr:Al:C molar ratio of 2:1 and 1:1, respectively. A 10 % excess of Al has been used due to its low melting point, which leads to a partial metal loss during the thermal process [35, 36]. The weighed elements have been placed in grinding containers (bowl and balls made of zirconium oxide) under an argon atmosphere and then ground for 3 h in a high-energy ball mill (Pulverisette 7, Fritsch, Idar-Oberstein, Germany) to obtain a homogeneous mixture with fragmented grains. The grinding has been performed in 12 cycles, with each cycle comprising 15 min of grinding at 300 rpm and 15 min of rest. After grinding, pellets with a diameter of 1 cm have been produced from the powders using a laboratory press with hydraulic pump for tablets (MP150, Maassen GmbH, Germany). The samples have been treated using ultra-high-pressure annealing (UHPA) technology [37]. The pellets have been placed in a graphite crucible and separated by graphite spacers. Annealing has been carried out for 15 hours at 1450 °C and under an argon pressure of 100 MPa. The heating and cooling rate have been 600 °C/h.

Structural Characterization

Diffraction studies have been performed in order to confirm the synthesis of Cr2AlC\mathrm{Cr}_{2}\mathrm{AlC} using a SuperNova diffractometer (Rigaku, Yarnton, Oxfordshire, UK) equipped with a CCD detector working with CuKα1_{\alpha1} (λ=1.54056\lambda= 1.54056 Å) radiation source and operating at 50 kV and 0.8 mA. The sample-to-detector distance has been 150 mm and the diffractograms have been recorded in the range of 10-120 2Theta. The sample images have been taken with a scanning electron microscope (SEM, Inspect S50, FEI Company, Hillsboro, Oregon, USA) equipped with a tungsten source and operating at 10 kV. Transmission electron microscopy (TEM, FEI Company, Tecnai T20 G2 XTWIN, Hillsboro, OR, USA) operating at 200 kV and equipped with a LaB6_{6} source has been also used. The sample has been placed on a 400-mesh copper grid covered with a film of holey carbon. To determine the elemental composition of the samples, the x-ray energy dispersion (EDX) spectroscopy measurement has been performed using an EDAX DPP-II analyzer installed on TEM.

Magnetic measurements

Magnetic measurements have been carried out using a Quantum Design MPMS XL superconducting quantum interference device (SQUID) magnetometer equipped with the reciprocating sample option (RSO) to enhance the signal-to-noise ratio. All experiments have been conducted following established protocols for high-precision and high-sensitivity integral SQUID magnetometry to ensure accurate determination of weak magnetic signals, minimize experimental artifacts, and guarantee full traceability of the measured magnetic response [38].

Measurements are performed over the full temperature range of 2 – 400 K, employing two distinct setups optimized for different thermal conditions. For temperatures up to approximately 340 K, the sample, a powdered material, has been enclosed in a standard polycarbonate capsule placed inside an in-situ compensating sample holder, which significantly suppresses the magnetic background signal originating from the capsule [39]. Specifically, the signal from an empty capsule with a typical mass of about 34 mg reduces to the equivalent of approximately 1 mg, yielding a background suppression factor of ~30, making it small in a comparison to a response of the powdered sample, which amounts to 192 mg, significantly simplifying the analysis.

Illumination-dependent magnetometry is performed using a custom prepared setup. All relevant technical details, including the holder geometry, sample preparation, wiring, measurement mode and thermal stability tests, are provided in the Supplementary Information (SI), Sec. S1 (including references [40, 41, 42, 43, 44]).

ESR Measurements

The Cr2_{2}AlC samples for the ESR measurements have been prepared as follows: A sample of a measured amount (1 mg) has been bounded to a polyethylene terephthalate (PET) substrate using adhesive. The PET substrate with the sample has been then placed in a sample tube. After evacuating the air, the tube has been filled with helium gas and sealed. ESR measurements have been taken using an X-band ESR spectrometer (JES-FA200; JEOL) at room temperature and 4 K. The gg-factor, the line width between a spectral peak and valley (ΔHpp\Delta H_{\mathrm{pp}}), and the number of spins (NspinN_{\mathrm{spin}}) have been calibrated based on the signals of a Mn2+^{2+} standard sample. The measurement sample has been placed in the center of the ESR cavity resonator, and the Mn2+^{2+} standard sample has been placed on the inner wall of the same ESR cavity resonator. The measurement and standard samples have been spatially separated and measured simultaneously in the same ESR cavity resonator. The temperature of the measurement sample has been variable. On the other hand, the temperature of the Mn2+^{2+} standard sample has been room temperature. The NspinN_{\mathrm{spin}} of the Mn2+^{2+} marker sample has been calibrated in advance using another standard sample 4-hydroxy-2,2,6,6-tetramethylpiperidin-1-oxyl (TEMPOL) solution [45, 46]. Simulated solar irradiation (AM1.5G) with a 100 mW cm−2^{-2} intensity has been used for the ESR measurements under light irradiation using a solar simulator (ONTOSOUN-150LX; Bunkoukeiki Co., Ltd.). The scheme of the ESR setup is presented in Figure 1.

Scheme of the ESR measurement setup, showing the ESR sample tube, He exchange gas, Mn$^{2+}$ marker, simulated solar irradiation (Xenon lamp), ESR sample, thermocouple, quartz double tube, ESR cavity, and He gas flow

Figure 1. Scheme of the ESR measurement setup.

Theoretical Tools

Properties of the ground state such as the band structure, magnetic states and Bloch functions have been calculated with the density functional theory (DFT) [47, 48] using the Quantum ESPRESSO package [49]. The generalized gradient approximation (GGA) has been chosen according to the Perdew-Burke-Ernzerhoff parameterization for the exchange-correlation functional [50]. Norm-conserving pseudopotentials have been used, with the energy cutoff for the plane waves set to 60 Ry. The first Brillouin zone (BZ) has been sampled using the uniform Monkhorst-Pack grid [51] with the kk-point mesh of 12×12×412 \times12 \times4.

Excitonic properties have been obtained from the solution of the ab initio BSE (ai-BSE) [52] implemented in the ab initio many-body perturbation theory (ai-MBPT) code called Yambo [53, 54]. The ai-BSE explicitly includes the electron-hole (e-h) correlations and takes the eigenvalues and eigenvectors of the DFT solution as building blocks of the perturbed Hamiltonian that describes the excited states. Tamm-Dancoff approximation has been used due to the computational complexity [55]. The e-h space contains 8 bands. The number of orbitals for the polarization function has been more than twice the number of electrons in the system. The plane waves have been used up to the energies of 10 Ry for the exchange components, 6 Ry for the screening and 4 Ry for response block size.

The bands interpolation has been done with the DFT Hamiltonian representation in the basis of the MLWF [56, 57] using the wannier90 code [58]. Detailed analysis of the spin-bands involved in the optical transitions has been performed by careful examination of their composition with respect to the MLWF centered at the Cr atoms.

Results and Discussion

Characterization of the crystal structure and calculations of the ground state properties

The Cr2_2AlC MAX phase occurs in the hexagonal crystal structure with the space group P63_3/mmc [59], and its Cr2_2C and Al layers are presented in Figure 2a for the side view and top view. Carbon atoms are 6-fold coordinated by three Cr atoms in the layers above and below the C layer, and this builds the sp3^3d2^2 hybridization around C involving electrons from the 3d shell of Cr.

Crystal structure of Cr2AlC and SEM images before and after heating

Figure 2. Crystal structure of Cr2AlC\mathrm{Cr}_{2}\mathrm{AlC}. a) Atomic structure: side and top views for the periodic repetition of the elementary unit cell. Color legend: C – grey, Cr – green, Al – orange. b) Elementary cell with the 3D map of spin distribution, positive in red and negative in blue. c) SEM image of milled precursors mixture before heating. d) SEM image of synthesized Cr2AlC\mathrm{Cr}_{2}\mathrm{AlC} product after heating.

The DFT calculations lead to the metallic ground state with the energetically close magnetic phases: paramagnetic (PM), antiferromagnetic (AF) and ferromagnetic (FM), which are summarized in Table S1 in SI. Results depend on the parametrization of the exchange-correlation functional, pseudopotentials and used geometry with the experimental lattice parameters or these theoretically calculated. This means in practice that coexistence of phases at low temperatures is very likely. The AF order develops in Cr2_2C layers, with the local magnetic moment at each Cr of ~1 μB\mu_{\mathrm{B}} and the absolute value of the magnetic moment in the elementary cell, containing two Cr2C\mathrm{Cr}_{2}\mathrm{C} layers, is close to 5 μB\mu_{\mathrm{B}}. Some partial spin moments are localized at Al atoms and their orientations are opposite to the magnetic moments at the adjacent Cr. Localization of the most pronounced positive and negative magnetic moments in the elementary cell is presented in Figure 2b that presents the 3D maps of the spin polarization in the AF phase.

ΔE=EX−EPM\Delta E=E_{\mathrm{X}}-E_{\mathrm{PM}}, X=AF, FM (Mtot/MabsM_{\mathrm{tot}}/M_{\mathrm{abs}})
geometryexperimentalrelaxed lattice parameters
PBE, noSOC, Cr PP with 6 valence electrons
AF-107 (0.0/5.06)-64 (0.0/4.98), a=2.912a=2.912, c=12.927c=12.927
FM-117 (3.40/4.23)-78 (3.37/4.15), a=2.897a=2.897, c=12.950c=12.950
PZ, both noSOC and SOC, Cr PP with 6 valence electrons
AF/FMConverges to PM
PBE, noSOC, Cr PP with 6 valence electrons, Hubbard Ueff=1U_{\mathrm{eff}}=1 eV at Cr-3d
AF-878 (0.0/10.11)-1155 (0.0/11.08), a=3.024a=3.024, c=13.061c=13.061
FM-555 (5.80/7.50)-530 (6.13/7.96), a=2.947a=2.947, c=12.950c=12.950
PZ, noSOC, Cr PP with 6 valence electrons, Hubbard Ueff=1U_{\mathrm{eff}}=1 eV at Cr-3d
AF-184 (0.0/5.86)-0.02 (0.0/4.16), a=2.853a=2.853, c=12.711c=12.711
FM-169 (3.48/4.33)-42 (3.33/4.01), a=2.843a=2.843, c=12.742c=12.742
PBE, SOC, Cr PP with 14 valence electrons
AFConverge to PM
FM-116 (3.43/4.22)-9 (3.14/3.72), a=2.851a=2.851, c=12.776c=12.776
PBE, noSOC, Cr PP with 14 valence electrons
AFConverges to PM
FM-117 (3.43/3.23)-8 (3.14/3.72), a=2.851a=2.851, c=12.774c=12.774

Table S1.

Results of the Cr2AlC\mathrm{Cr}_{2}\mathrm{AlC} synthesis are shown in SEM images. Figure 2c and Figure 2d present the powder mixture before and after heating, respectively, indicating a transformation of the material structure as a result of the thermal treatment. The SEM image of the product clearly confirms the layered structure that is characteristic for the MAX phase [59, 60, 61, 62].

After the synthesis, the obtained material has been characterized. The x-ray diffractograms of the precursor mixture after milling, the synthesized product, and the Cr2AlC\mathrm{Cr}_{2}\mathrm{AlC} reference (PDF Card 290017) are shown in Figure 3a. Although carbon remains in the mixture after milling, no reflections characteristic of graphite have been observed. This is because grinding destroys its ordered structure leading to a formation of an amorphous phase. The diffractogram for the milled sample shows reflections corresponding to the hklhkl planes: (111), (200), (220), (311), (222), (400), (331), (420) for aluminium (PDF Card 040787) and (110), (200), (211), (220) and (310) for chromium (PDF Card 060694), respectively. The diffractograms show no additional reflections. This proves that grinding has no effect on the chemical composition of the mixture and no side processes occur during it. The diffraction pattern obtained for the synthesized Cr2AlC\mathrm{Cr}_{2}\mathrm{AlC} product is consistent with the PDF Card 290017 standard. Characteristic reflections for the Cr2AlC\mathrm{Cr}_{2}\mathrm{AlC} MAX phase have been observed at: 13.8, 27.9, 36.2, 36.9, 42.1, 42.2, 46.3, 56.9, 65.2, 77.1, 80.8, 111.0 and 114.8 2 Theta corresponding to the hklhkl lattice planes: (002), (004), (100), (101), (103), (006), (104), (106), (110), (109), (116), (209) and (213), respectively. This confirms that we obtain the MAX phase in the hexagonal crystal structure with the space group P63/mmcP6_{3}/mmc [59, 60]. The diffraction pattern shows additional, very low-intensity reflections marked with an asterisk, indicating the formation of a very small amount of impurities from other phases such as Al2O3\mathrm{Al}_{2}\mathrm{O}_{3} or Cr7C3\mathrm{Cr}_{7}\mathrm{C}_{3}.

Characterization of Cr2AlC

Figure 3. Characterization of Cr2_2AlC. a) X-ray diffractograms of the milled precursors mixture (blue), synthesize product (black) and standard Cr2_2AlC PDF Card 290017 (green). b) HRTEM images of Cr2_2AlC. c) FFT images obtained for the surface marked with a red frame in the corresponding HRTEM images. d) IFFT images obtained for the surface marked with a red frame in the corresponding HRTEM images. e) EDX profile for the synthesized Cr2_2AlC.

The high resolution TEM (HRTEM) images of the synthesised sample, presented in Figure 3b, demonstrate the presence of well organised areas of the crystal structure. The Fast Fourier Transform (FFT), presented in Figure 3c, and Inverse Fast Fourier Transform (IFFT), presented in Figure 3d, have been done for the red-framed regions of the HRTEM images, and both analyses correspond to the two crystal directions. These characterization techniques reveal that the distances between planes are of 0.641 nm and 0.248 nm corresponding to the (002) and (100), respectively, lattice planes of the hexagonal Cr2_2AlC [61, 62]. The EDX study, presented in Figure 3e, definitively shows the presence of chromium, aluminium and carbon in the Cr2_2AlC sample. Additionally, the Cu peak comes from the copper mesh on which the sample is placed, while the small Si peak originates from the EDX Si-Li detector. In conclusion, structural and morphological studies confirm the efficiency of the synthesis of Cr2_2AlC.

Magnetic properties obtained with SQUID

The material exhibits clear paramagnetic properties in the whole studied temperature range as exemplified in Figure 4. At 300 K the magnetization MM is strictly linear in field within experimental accuracy, as presented in Figure 4a, with a mass susceptibility χ=3.5(1)×10−6\chi=3.5(1)\times10^{-6} emu/g/Oe. Since the diamagnetic component of Cr2_2AlC estimated from Pascal constants amounts to χdia≃5×10−7\chi_{\mathrm{dia}} \simeq5\times10^{-7} emu/g/Oe [63], we obtain the Cr-related susceptibility χCr\chi_{\mathrm{Cr}}(300 K) of 4.0(2)×10−64.0(2)\times10^{-6} emu/g/Oe. The corresponding magnetization at 10 kOe is MCrM_{\mathrm{Cr}}(300 K) = 0.040(2) emu/g, which gives 5.1(3)×10−45.1(3)\times10^{-4} μB\mu_{\mathrm{B}} per Cr atom, or 1.0(1)×10−31.0(1)\times10^{-3} μB\mu_{\mathrm{B}} per Cr2_2AlC formula unit.

Magnetization and magnetic susceptibility of Cr2AlC

Figure 4. a) Magnetization of the Cr2AlC\mathrm{Cr}_{2}\mathrm{AlC} powder as a function of magnetic field HH, measured at 300 K using the capsule compensating sample holder (CCSH) – full symbols – versus a test measurement of the empty capsule in the same CCSH – grey open symbols. b) Temperature dependence of the magnetic susceptibility χCr\chi_{\mathrm{Cr}} of Cr subsystem in Cr2AlC\mathrm{Cr}_{2}\mathrm{AlC}: Orange squares – as measured, brown full circles – after removing the Curie paramagnetism; details are given in SI, Sec. S3. The horizontal dotted line marks the magnitude of the Pauli paramagnetism after correction for the core diamagnetism of the constituent atoms, χdia≅5×10−7\chi_{\mathrm{dia}} \cong5 \times10^{-7} emu/g/Oe [65]. Full red diamonds mark the remaining TT-dependent part of χCr\chi_{\mathrm{Cr}}, evaluated in the view of AF coupled Cr-Cr dimers and represented by the black thick dashed line.

Such a small, field-linear response is characteristic for Pauli paramagnetism of conduction electrons, χP\chi_{\mathrm{P}}, and represents the dominant magnetic component in Cr2AlC\mathrm{Cr}_{2}\mathrm{AlC}. This assignment is consistent with previous NMR and magnetometry studies that reported the Korringa-type relaxation and a weak temperature dependence of χ\chi over a broad range of temperatures [64]. While Van Vleck paramagnetism can also yield a temperature-independent term, it typically arises from localized ionic states with low-lying excited levels. This scenario is unlikely in a good metal like Cr2AlC\mathrm{Cr}_{2}\mathrm{AlC} where hybridized Cr-3d states form itinerant bands at the Fermi level. Additionally, we note that no signatures of long-range magnetic order are detected what signifies a single magnetic constitution of the material synthetized for this studies.

On the other hand, as depicted in Figure 4b by orange squares, the measured magnetic susceptibility χ(T)=M(T)/H\chi(T) = M(T)/H (with H=10H = 10 kOe) reveals three distinct contributions which all together reproduce the overall temperature dependence. Listing in order of magnitude, these contributions are as follows: The first consists of two temperature-independent components discussed above, namely the Pauli paramagnetic susceptibility χP\chi_{\mathrm{P}} and the core diamagnetism of the constituent atoms χdia\chi_{\mathrm{dia}}. Their summation forms the temperature-independent baseline of χ(T)\chi(T), marked by the thin black line in Figure 4b. The second contribution is a Curie-type upturn that develops below 100 K. The third component is the term that increases with temperature and tends to saturate above 400 K.

The low-TT paramagnetic component, χPM(T)\chi_{\mathrm{PM}}(T), is ubiquitously observed in MAX-phase compounds [66, 67, 34]. We quantify χPM(T)\chi_{\mathrm{PM}}(T) using a differential Brillouin-function analysis of magnetization curves measured at temperature between 2 K and 8 K, as described in details in SI, Sec. S3 (including Figs. S3 and S4, and references 65 and 68-71). The analysis shows that this low-TT upturn originates from a very small concentration, approximately 0.02 %, of localized spins with S=3/2S = 3/2.

We attribute these localized spins to a small fraction of Cr sites in structurally or chemically distinct environments, where electronic delocalization is locally reduced and local moments can be stabilized. A minute population of such centers may arise from antisite defects, off-stoichiometric regions, locally distorted Cr environments, surface-oxidized layers, or grain-surface terminations. In a powder sample, the latter contribution may be enhanced by the distribution of grain surfaces, terminations and defect configurations. The sensitivity of Cr2AlC\mathrm{Cr}_{2}\mathrm{AlC} to such local perturbations is also consistent with the near degeneracy of several magnetic/electronic configurations predicted by DFT using different parametrizations, summarized in Table S1 in SI, Sec. S2.

Determination of χPM\chi_{\mathrm{PM}} allows us to isolate the temperature-independent contribution to the total susceptibility, χP+χdia\chi_{\mathrm{P}}+\chi_{\mathrm{dia}}, and thereby to extract the absolute value of the Pauli susceptibility χP≃3.3×10−6\chi_{\mathrm{P}} \simeq3.3 \times10^{-6} emu/g/Oe, as indicated by the dotted line in Figure 4b. Such a small χP\chi_{\mathrm{P}} is typical for MAX-phase compounds and other metallic systems, and enables even a very little concentration of localized paramagnetic spins to become discernible at low temperatures. In our sample, the χPM\chi_{\mathrm{PM}} term contributes only by about 1 % to the total χ\chi at 300 K, and thus has no significant influence on the room-temperature magnetic response. Therefore it can be neglected in the following discussion.

The remaining TT-dependent component of χCr(T)\chi_{\mathrm{Cr}}(T), indicated by the solid red diamonds in Figure 4b, cannot be described by a simple Curie-Weiss or Pauli term. Notably, in the previous high-temperature study of Cr2AlC\mathrm{Cr}_{2}\mathrm{AlC} up to 800 K, a broad maximum of χ(T)\chi(T) centered around 350 - 400 K was observed [34]. In agreement with that report, our measurements also show the increase of χ(T)\chi(T) with temperature, although with a progressively reduced slope above 300 K suggesting that a similar maximum may occur in our sample at temperatures above 400 K, which is beyond our experimental limit.

Such a characteristic temperature dependence of the magnetic susceptibility can be analyzed using the Bleaney-Bleaney (B-B) model for exchange-coupled dimers, i.e. a binuclear spin system described by the isotropic exchange Hamiltonian H=−2J S1⋅S2H = -2J\,\mathbf{S}_{1}\cdot\mathbf{S}_{2}, where JJ is the exchange coupling constant between the two spins. In this convention, antiferromagnetic coupling corresponds to J<0J < 0; below we therefore discuss the coupling strength through the positive energy scale ∣J∣/kB\lvert J\rvert/k_{\mathrm{B}}. In this framework, two Cr ions, each carrying S=1/2S = 1/2, form antiferromagnetically coupled pairs with a singlet ground state (Stot=0S_{\mathrm{tot}} = 0) and a thermally populated triplet excited state (Stot=1S_{\mathrm{tot}} = 1). Accordingly, the residual χCr(T)\chi_{\mathrm{Cr}}(T) is fitted with the expression:

χB−B(T)=(C/T)⋅[2/(3+e∣J∣/kBT)](1)\chi_{\mathrm{B-B}}(T) = (C/T) \cdot\left[2/(3 + e^{\lvert J\rvert/k_{\mathrm{B}}T})\right] \tag*{(1)}

where the term in square brackets is a dimensionless statistical factor representing the Boltzmann-weighted thermal population distribution among the spin multiplet states [72, 73]. The least-squares fit of Eq. (1), marked by the thick dashed line in Figure 4b, yields an exchange energy of J/kB=760(10)J/k_{\mathrm{B}} = 760(10) K and the Curie constant C=Nd⋅(gμB)2/kB=1.60(2)×10−3C = N_{\mathrm{d}}\cdot(g\mu_{\mathrm{B}})^2/k_{\mathrm{B}} = 1.60(2) \times10^{-3} emu·K/g/Oe. Here, NdN_{\mathrm{d}} denotes the number of Cr-Cr dimers per gram of sample. To express this value as a fraction of the Cr sublattice, we define ξ=2 Nd/NCr=Nd/Nf.u.\xi= 2\,N_{\mathrm{d}}/N_{\mathrm{Cr}} = N_{\mathrm{d}}/N_{\mathrm{f.u.}}, where NCrN_{\mathrm{Cr}} and Nf.u.N_{\mathrm{f.u.}} are the numbers of Cr atoms and Cr2AlC\mathrm{Cr}_{2}\mathrm{AlC} formula units per gram, respectively. The fitted dimer density Nd=6.4(2)×1020N_{\mathrm{d}} = 6.4(2) \times10^{20}/g therefore corresponds to ξ=0.15(1)\xi= 0.15(1), meaning that about 15% of Cr ions participate in antiferromagnetically coupled dimers.

Deduced spin value S=1/2S = 1/2 is consistent with the values of Cr spin polarization obtained from the DFT of about 1 μB1\,\mu_{\mathrm{B}}. This value may be slightly underestimated by the DFT owing to its approximate treatment of the electron correlations and a way of partitioning a crystal to atoms. Formal oxidation state of Cr in Cr2AlC\mathrm{Cr}_{2}\mathrm{AlC} is not uniquely defined, a one-to-one correspondence between an ionic configuration and the observed spin state cannot be established [74].

Thus, the main magnetic response is ascribed to a weak metallic Pauli-like susceptibility modified by a sizeable dimer-like antiferromagnetic contribution. By contrast, the dilute Curie-like component represents only a minute fraction of Cr sites and is relevant mainly for the low-temperature upturn. This separation of scales motivates two complementary normalizations of the conduction-related parameters. The conventional sample-averaged normalization describes the macroscopic response of Cr2AlC\mathrm{Cr}_{2}\mathrm{AlC} as measured, whereas the active-fraction normalization excludes the Cr fraction involved in the dimer-like contribution and therefore estimates the electronic density of states associated with the remaining itinerant subsystem. The resulting parameters are summarized in Table 1, where the two normalization schemes are compared.

QuantitySymbol (unit)Sample-averaged (factive=1.00f_{\mathrm{active}} = 1.00)Active-fraction normalized (factive=0.85f_{\mathrm{active}} = 0.85)
Molar susceptibilityχm\chi_m (cm3^3/mol)4.7(1)×10−44.7(1) \times10^{-4}5.5(1)×10−45.5(1) \times10^{-4}
Effective density of states for both spinsEDOS⁡(EF)\operatorname{EDOS}(E_F) (states⋅\cdoteV−1⋅^{-1}\cdotf.u.−1^{-1})15(1)17(1)
Effective density of states per Cr atomEDOS⁡(EF)/Cr\operatorname{EDOS}(E_F)/\mathrm{Cr} (states⋅\cdoteV−1⋅Cr−1^{-1}\cdot\mathrm{Cr}^{-1})7(1)10(1)

Table 1. Material parameters derived from the Pauli susceptibility differentiating two different approaches for the whole sample and only its metallic part (assuming active-fraction factive=1−ξ=0.85f_{\mathrm{active}} = 1-\xi= 0.85). The values given for the effective density of states (EDOS) at the Fermi level, EDOS⁡(EF)=χP/μB2\operatorname{EDOS}(E_F) = \chi_P/\mu_B^2, indicate their upper limits in Cr2AlC\mathrm{Cr}_2\mathrm{AlC}.

Illumination-dependent SQUID magnetometry was also performed to test whether the low-temperature magnetic response of Cr2AlC\mathrm{Cr}_2\mathrm{AlC} can be modified optically. No measurable intrinsic optomagnetic response was detected under red-LED illumination (610 nm) down to 2 K. Even at the highest LED current used, the only observable change was a small reversible shift of M(T)M(T) consistent with illumination-induced heating, as documented in SI, § 9.

Optomagnetic properties obtained with ESR measurements and BSE calculations

ESR measurements are first performed on a powder sample of Cr2AlC\mathrm{Cr}_2\mathrm{AlC} at room temperature. No ESR signal has been detected either in the dark or under light irradiation. To probe possible low-temperature magnetic centers, ESR measurements are then carried out at 4 K. As shown in Figure 5a, a clear ESR signal with a gg-factor of 2.0038 is observed in the dark state. Calibration against the Mn2+\mathrm{Mn}^{2+} standard gives Nspin=3.80×1017N_{\mathrm{spin}} = 3.80 \times10^{17} spins per gram of Cr2AlC\mathrm{Cr}_2\mathrm{AlC}, which corresponds to only 0.0045% of all Cr sites. The peak-to-peak linewidth, ΔHpp\Delta H_{\mathrm{pp}}, is 0.92 mT. The ESR signals of the Mn2+\mathrm{Mn}^{2+} standard appear with the opposite phase to those of Cr2AlC\mathrm{Cr}_2\mathrm{AlC} because the microwave oscillating magnetic fields at the positions of the standard and the sample have opposite directions.

Change of the local magnetization due to light excitation

Figure 5. Change of the local magnetization due to light excitation. a) ESR signals of Cr2AlC\mathrm{Cr}_{2}\mathrm{AlC} at 4 K with experimental procedure: in the dark state – blue line, under light irradiated for 1 h – red line, in the dark state for 1 h after the irradiation – green line. b) Comparison of ESR signals presented in (a) and the background signal of the ESR cavity resonator – black line. In (a) and (b), ESR signals from the standard Mn2+\mathrm{Mn}^{2+} sample are shown. c) Scheme of the spin hopping, denoted by e↑\uparrow and e↓\downarrow, between the Cr atoms with the opposite local moments, denoted by Cr↑\uparrow and Cr↓\downarrow, induced by light absorption. d) Scheme of the MLWF-composition analysis of the spin-bands involved in the optical transitions. States below and above the Fermi level are denoted by G and E, respectively, first and second index are denoted spin and atomic-shell, respectively, and the change of local magnetization is denoted by ΔM\Delta M.

After 1 h of simulated solar irradiation, the ESR signal intensity decreases, the gg-factor changes from 2.0038 to 2.0051, and NspinN_{\mathrm{spin}} decreases to 8.58×10168.58 \times10^{16} spins per gram. At the same time, ΔHpp\Delta H_{\mathrm{pp}} increases to 1.32 mT. After switching off the irradiation, the signal intensity, gg-factor and linewidth return to their initial dark-state values, as shown in Figure 5b. The optically modified part of the ESR signal therefore corresponds to about 2.90×10172.90 \times10^{17} spins per gram, i.e. only ∼0.0035%\sim0.0035\% of all Cr sites. Thus, ESR reveals a reversible light-induced modification of a very dilute population of local magnetic centers in Cr2AlC\mathrm{Cr}_2\mathrm{AlC}, rather than a bulk optical switching of magnetism in the MAX phase.

A plausible microscopic mechanism for the reduction of the local ESR signal is light-induced redistribution of spin polarization between adjacent Cr sites. This scenario is schematically shown in Figure 5c. In regions where neighboring Cr atoms carry opposite local spin polarizations, optical excitation may transfer electronic weight from a majority-spin state localized on one Cr site to states with larger contribution from the neighboring Cr site with the opposite local moment. In this simplified picture, optical excitations from the ground state (G) to excited states (E) in a given spin channel modify the spatial distribution of spin polarization through the different atomic composition of the involved Bloch states, as illustrated in Figure 5d by the GijG_{ij} and EijE_{ij} components.

We are mostly interested in bands composition with respect to the Cr atoms, therefore we present the projections of the spin-bands up and down on the MLWF centered at two Cr with the local magnetic moments up and down in Figure 6. Definitions of the high symmetry points in the Brillouin zone (BZ) sampling for the hexagonal crystal structure are given in Table S2 in SI. For completeness, projections of the spin bands on the MLWF centered at Al and C are presented in Figure S5 in SI. Electrons from the atomic shells of Al and C do not contribute to the band structure in the energy region of ±2\pm2 eV below and above the Fermi level, thus being optically inactive.

Spin-bands projected at the MLWF centered at two Cr atoms with the local magnetization up and down

Figure 6. Spin-bands projected at the MLWF centered at two Cr atoms with the local magnetization up and down. Color legend is common for all cases and truncated to the range [0.3,0.7] for a better contrast. a) Bands for spin up projected at Cr with local magnetic moment up, Cr↑Cr^{\uparrow}. b) As in (a) for Cr with the local magnetic moment down, Cr↓Cr^{\downarrow}. c) and d) correspond to a) and b), respectively, for bands with spin down.

kk-point(u, v, w)(kxk_x, kyk_y, kzk_z)
Γ\Gamma(0, 0, 0)[0, 0, 0]
M(1/2, 0, 0)[π\pi/a, -π\pi/3\sqrt{3}a, 0]
K(2/3, 1/3, 0)[4π\pi/3a, 0, 0]
A(0, 0, 1/2)[0, 0, π\pi/c]
L(½, 0, 1/2)[π\pi/a, -π\pi/3\sqrt{3}a, π\pi/c]
H(2/3, 1/3, 1/2)[4π\pi/3a, 0, π\pi/c]

Table S2. List of the high symmetry points in the Brillouin zone (BZ) for the hexagonal crystal structure with the space group P63_3/mmc. The parameters aa and cc are the basal and vertical lattice parameters, respectively.

Spin-bands projected at maximally-localized Wannier functions for Al and C atoms, spin up and spin down

Figure S5. The spin-bands projected at the maximally-localized Wannier functions centered at: a) Al atoms for spin up, b) Al atoms for spin down, c) C atoms for spin up and d) C atoms for spin down. Color legend is common for all cases and truncated to the [0.0,0.6] range for a better contrast.

Examining closely the Γ\Gamma-AA high symmetry line in BZ in Figure 6a-Figure 6d: the majority spin-bands at each type of Cr (i.e. spin up for Cr↑Cr^{\uparrow} and spin down for Cr↓Cr^{\downarrow}) are localized below the Fermi level, while the minority spin-bands (i.e. spin down for Cr↑Cr^{\uparrow} and spin up for Cr↓Cr^{\downarrow}) are localized above the Fermi level. Similar situation is partially for MM-Γ\Gamma and LL-AA high symmetry lines. Thus, the direct optical excitations in these regions of the BZ would reduce the local magnetic moment at each Cr. In contrast, the opposite composition of the spin-bands is near the M point towards K and near the L point towards H, therefore the optical transitions in these regions would lower the local magnetic moments at Cr, while transitions near K would be neutral for a change of the local magnetization.

Each exciton consists of several nearly degenerate dipole transitions, i.e. band-to-band excitations at a given kk-point in BZ. Composition of bands involved in the optical transitions with respect to the atomic shells of four Cr atoms in the elementary cell indicates an effect of light absorption of given energy for a change of the local magnetization, which we define as

ΔM=∑Cr↑,Cr↓∑v,c∑kωk{[Ac↑,k(Cr↑)−Av↑,k(Cr↑)]−[Ac↓,k(Cr↑)−Av↓,k(Cr↑)]+[Ac↓,k(Cr↓)−Av↓,k(Cr↓)]−[Ac↑,k(Cr↓)−Av↑,k(Cr↓)]}(2)\Delta M = \sum_{Cr^{\uparrow},Cr^{\downarrow}} \sum_{v,c} \sum_k \omega_k \{[A_{c^{\uparrow},k}(Cr^{\uparrow}) - A_{v^{\uparrow},k}(Cr^{\uparrow})] - [A_{c^{\downarrow},k}(Cr^{\uparrow}) - A_{v^{\downarrow},k}(Cr^{\uparrow})] + [A_{c^{\downarrow},k}(Cr^{\downarrow}) - A_{v^{\downarrow},k}(Cr^{\downarrow})] - [A_{c^{\uparrow},k}(Cr^{\downarrow}) - A_{v^{\uparrow},k}(Cr^{\downarrow})]\} \tag*{(2)}

The coefficients AcA_c and AvA_v denote contributions of the MLWF centered at Cr to the conduction band, cc, and valence band, vv, and arrows in the subscript indicate the spin channel of the corresponding band while arrows near Cr indicate the local magnetic moment at a given atom. We sum this formula over all atoms with the same local magnetic moment, valence and conduction bands, and kk-points with their weights ωk\omega_k in BZ.

The normalized absorption spectra obtained from the ai\mathit{ai}-BSE for two light polarizations are presented in Figure 7a-Figure 7b, that contains also bars corresponding to the summed change of the local magnetization at all Cr atoms induced by excitons of a given energy. Thickness of these bars indicates the nearly degenerate optical transitions. Please note that the change of magnetization in a case of the light polarization [0,0,1], in Figure 7b, is plotted in units that are five times larger than those for the polarization [1,0,0], in Figure 7a. Effectiveness of the optical switching of local magnetic moment at a given wavelength depends on two factors: i) the number of nearly degenerate excitons and their oscillator strengths and ii) the favorite compositions, with respect to the Cr atomic shells, of the spin bands involved in the dipole transitions. In order to give a full picture of the optomagnetic effects, we include additional data in SI: 1) the absolute (not normalized) absorption spectra for the [1,0,0] and [0,0,1] polarizations are presented in Figure S6, 2) the list of kk-points used in the irreducible wedge of BZ is in Table S3, and 3) the list of excitons with the oscillator strengths larger than 0.1 is given in Table S4 including the order number of given exciton in the spectrum and composition of the main dipole transitions found in the corresponding eigenvectors (it means the order numbers of involved bands, their spin channel and kk-point), as well as the change of the local magnetic moment at all Cr in the cell induced by the proper dipole transition, 4) the comparative plot of light-induced local magnetic moments with respect to the light energy and the exciton oscillator strengths, in Figure S7, for both light polarizations: a) [1,0,0] and b) [0,0,1]. Taking into account all data, we summarize, that the most effective parts of light absorption for switching the magnetic moment are: 1) the very low-energy spectrum (THz frequencies) with the Cr2_2C in-plane polarization (i.e. crystal direction [1,0,0] and the symmetry equivalent [0,1,0]) due to high oscillator strengths and magnetization-reducing effect, and 2) the infrared part of the spectrum (near 1200 nm) for the light polarization along the crystal cc-axis (i.e. crystal direction [0,0,1]) due to the reversed spin-band compositions with respect to the majority spin at the Cr atoms.

Normalized absorption spectra and change of local magnetization for two electric-field vectors

Figure 7. The normalized absorption spectrum obtained from the ai\mathit{ai}-BSE (blue line) and change of the local magnetization at all Cr atoms induced by an exciton of given energy (red bars) for the electric-field vectors: a) [1,0,0] and b) [0,0,1]. Color arrows point to the proper axis at each plot.

Figure S6. Comparison of the not normalized absorption spectra obtained from the solution of ai-BSE with the electric field vector oriented along the [1,0,0] and [0,0,1] crystal directions.

No.Cartesian coordinates in units 2π/a2\pi/a (a is the lattice constant = 5.4983 a.u.)Crystal coordinates
10.0000000 0.0000000 0.00000000.0000000 0.0000000 0.0000000
20.0000000 0.0000000 0.05629850.0000000 0.0000000 0.2500000
30.0000000 0.0000000 -0.11259710.0000000 0.0000000 -0.5000000
40.0000000 0.0963226 0.00000000.0000000 0.0833333 0.0000000
50.0000000 0.0963226 0.05629850.0000000 0.0833333 0.2500000
60.0000000 0.0963226 -0.11259710.0000000 0.0833333 -0.5000000
70.0000000 0.1926452 0.00000000.0000000 0.1666667 0.0000000
80.0000000 0.1926452 0.05629850.0000000 0.1666667 0.2500000
90.0000000 0.1926452 -0.11259710.0000000 0.1666667 -0.5000000
100.0000000 0.2889678 0.00000000.0000000 0.2500000 0.0000000
110.0000000 0.2889678 0.05629850.0000000 0.2500000 0.2500000
120.0000000 0.2889678 -0.11259710.0000000 0.2500000 -0.5000000
130.0000000 0.3852905 0.00000000.0000000 0.3333333 0.0000000
140.0000000 0.3852905 0.05629850.0000000 0.3333333 0.2500000
150.0000000 0.3852905 -0.11259710.0000000 0.3333333 -0.5000000
160.0000000 0.4816131 0.00000000.0000000 0.4166667 0.0000000
170.0000000 0.4816131 0.05629850.0000000 0.4166667 0.2500000
180.0000000 0.4816131 -0.11259710.0000000 0.4166667 -0.5000000
190.0000000 -0.5779357 0.00000000.0000000 -0.5000000 0.0000000
200.0000000-0.57793570.05629850.0000000-0.50000000.2500000
210.0000000-0.5779357-0.11259710.0000000-0.5000000-0.5000000
220.08341780.14448390.00000000.08333330.08333330.0000000
230.08341780.14448390.05629850.08333330.08333330.2500000
240.08341780.1444839-0.11259710.08333330.0833333-0.5000000
250.08341780.24080650.00000000.08333330.16666670.0000000
260.08341780.24080650.05629850.08333330.16666670.2500000
270.08341780.2408065-0.11259710.08333330.1666667-0.5000000
280.08341780.33712920.00000000.08333330.25000000.0000000
290.08341780.33712920.05629850.08333330.25000000.2500000
300.08341780.3371292-0.11259710.08333330.2500000-0.5000000
310.08341780.43345180.00000000.08333330.33333330.0000000
320.08341780.43345180.05629850.08333330.33333330.2500000
330.08341780.4334518-0.11259710.08333330.3333333-0.5000000
340.08341780.52977440.00000000.08333330.41666670.0000000
350.08341780.52977440.05629850.08333330.41666670.2500000
360.08341780.5297744-0.11259710.08333330.4166667-0.5000000
370.16683570.28896780.00000000.16666670.16666670.0000000
380.16683570.28896780.05629850.16666670.16666670.2500000
390.16683570.2889678-0.11259710.16666670.1666667-0.5000000
400.16683570.38529050.00000000.16666670.25000000.0000000
410.16683570.38529050.05629850.16666670.25000000.2500000
420.16683570.3852905-0.11259710.16666670.2500000-0.5000000
430.16683570.48161310.00000000.16666670.33333330.0000000
440.16683570.48161310.05629850.16666670.33333330.2500000
450.16683570.4816131-0.11259710.16666670.3333333-0.5000000
460.16683570.57793570.00000000.16666670.41666670.0000000
470.16683570.57793570.05629850.16666670.41666670.2500000
480.16683570.5779357-0.11259710.16666670.4166667-0.5000000
490.25025350.43345180.00000000.25000000.25000000.0000000
500.25025350.43345180.05629850.25000000.25000000.2500000
510.25025350.4334518-0.11259710.25000000.2500000-0.5000000
520.25025350.52977440.00000000.25000000.33333330.0000000
530.25025350.52977440.05629850.25000000.33333330.2500000
540.25025350.5297744-0.11259710.25000000.3333333-0.5000000
550.33367130.57793570.00000000.33333330.33333330.0000000
560.33367130.57793570.05629850.33333330.33333330.2500000
570.33367130.5779357-0.11259710.33333330.3333333-0.5000000
580.0000000-0.09632260.05629850.0000000-0.08333330.2500000
590.0000000-0.19264520.05629850.0000000-0.16666670.2500000
600.0000000-0.28896780.05629850.0000000-0.25000000.2500000
610.0000000-0.38529050.05629850.0000000-0.33333330.2500000
620.0000000-0.48161310.05629850.0000000-0.41666670.2500000
63-0.0834178-0.24080650.0562985-0.0833333-0.16666670.2500000
64-0.0834178-0.33712920.0562985-0.0833333-0.25000000.2500000
65-0.0834178-0.43345180.0562985-0.0833333-0.33333330.2500000
66-0.0834178-0.52977440.0562985-0.0833333-0.41666670.2500000
67-0.1668357-0.38529050.0562985-0.1666667-0.25000000.2500000
68-0.1668357-0.48161310.0562985-0.1666667-0.33333330.2500000
69-0.2502535-0.52977440.0562985-0.2500000-0.33333330.2500000

Table S3. The list of k-points in the irreducible symmetry wedge of BZ (IBZ) used for solving the ab initio BSE with the use of the uniform mesh of the 12×12×412 \times12 \times4 grid.

EXE_{\mathrm{X}} (eV)ffNo.bvalb_{\mathrm{val}}bcondb_{\mathrm{cond}}kkspinΔM\Delta M
Electric field vector [1,0,0]
0.038960280.4337255
0.038960820.7144256
0.039005571.000025945469U D-0.113
0.039008390.6842260424318U D-0.026
0.039547670.4273268
0.039552890.8781269
0.039600370.7446271
0.039604560.7899272
0.042721380.239128745465U D-0.036
0.042736180.1863289454658U D-0.069
0.043106560.2313298
0.049102490.3118334
0.049165310.3645337
0.049166050.213833844469U D-0.105
0.049963060.1986340
0.049965480.2612341
0.050029710.4124343
0.050032830.1919344
0.063415200.231240645464U D-0.044
0.063443530.1774410424316U D-0.035
0.063886430.2000413
0.089326260.1310590444523U D-0.083
0.089341130.5461591
0.089386970.427760045468U D-0.139
0.089393090.1330601454659U D-0.158
0.089798030.6369608
0.089997980.2048610
0.090002400.7790611
0.090085690.4336614
0.090423320.1561619
0.090425660.2242620
0.132295940.101589845467U D-0.170
0.132333910.2847901
0.132954640.2160904
0.133007200.2131907
0.210257260.14421508414235U D-0.244
0.210259960.12831509414266U D-0.252

Table S4. The list of excitons and contributing dipole transitions (i.e. band-to-band excitations at given kk-point in BZ): energy of the exciton (EXE_{\mathrm{X}}), oscillator strength (ff), number of the given excitation in the whole spectrum, dominant excitations from the occupied band (bvalb_{\mathrm{val}}) to the unoccupied band (bcondb_{\mathrm{cond}}) at the corresponding kk-point in BZ (according to the list in Table S2) and the spin channel (up denored “U” and/or down denoted “D”) that causes a change of the local magnetization (ΔM\Delta M). The weights of the listed band-to-band contributions are larger than 5%.

Figure S7. Normalized oscillator strengths (in blue color) of the dipole transitions in the absorption spectrum obtained from the solution of ab initio BSE with the electric-field vector oriented along: a) the [1,0,0]\left[1,0,0\right] crystal direction and b) [0,0,1]\left[0,0,1\right] crystal axis. The corresponding change of the local magnetization in the elementary cell (in red color) caused by the dominant excitations are given for the transitions with the oscillator strength threshold >0.1> 0.1.

Conclusion

In this work, we synthesized the Cr2_2AlC MAX phase by annealing pellets prepared from elemental powders for 15 h at 1450 °C under an Ar pressure of 100 MPa, using heating and cooling rates of 600 °C/h. The obtained material was characterized by x-ray diffraction, energy-dispersive x-ray spectroscopy, scanning electron microscopy, and high-resolution transmission electron microscopy.

Magnetometry identifies Cr2AlC\mathrm{Cr}_{2}\mathrm{AlC} as a weak, field-linear paramagnet over the investigated temperature range, with the dominant response assigned to the Pauli-like susceptibility of itinerant Cr-derived states. The temperature dependence is, however, not purely metallic. After separating a trace low-temperature Curie-like contribution from dilute localized Cr centers, the remaining non-monotonic susceptibility is consistently described by antiferromagnetically coupled Cr-Cr dimers. The sizeable dimer-like fraction inferred from the Bleaney-Bowers analysis indicates that local antiferromagnetic correlations involve a non-negligible part of the Cr sublattice, although no macroscopic long-range magnetic order has been detected.

Illumination-dependent magnetometry using red-light excitation did not reveal an intrinsic macroscopic optomagnetic response within the experimental sensitivity. At the highest light intensity used, the only detectable change of the magnetic moment can be consistent with a small reversible heating of the sample environment.

These results are complementary to ESR measurements and DFT and ai-BSE calculations. ESR measurements at 4 K reveal a local magnetic signal that is strongly reduced under illumination and recovers in the dark. Its mechanism can be ascribed by the ai-BSE solution and the MLWF analysis as a spin excitation from Cr to the neighboring Cr atom. Importantly, the optically modified ESR signal corresponds only to several tens of ppm of the Cr sublattice. Thus, ESR detects a highly light-sensitive but extremely dilute population of local magnetic centers, whereas the overwhelming majority of Cr sites does not contribute to the detected optical switching. This naturally explains why the corresponding effect is not resolved as a macroscopic magnetization change in the magnetometry.

DFT calculations point to a metallic state with closely competing magnetic configurations, including paramagnetic and antiferromagnetic solutions. Taken together, the results suggest that Cr2AlC\mathrm{Cr}_{2}\mathrm{AlC} is not a conventional long-range ordered magnet, but a metallic system close to local magnetic instabilities. In this picture, itinerant Cr-derived states coexist with local antiferromagnetic Cr-Cr correlations and a trace concentration of localized paramagnetic centers. The optical sensitivity observed by ESR should therefore be understood as a local magnetic/electronic response of these rare centers rather than as a bulk optomagnetic switching of the Cr2AlC\mathrm{Cr}_{2}\mathrm{AlC} phase.

Declaration of Competing Interest

The authors declare that they have no known competing financial interests or personal relationships that could have appeared to influence the work reported in this paper.

Acknowledgements

We gratefully acknowledge Poland’s high-performance infrastructure PL-Grid in the Cyfronet Center for providing computer facilities and support within the computational grants No. PLG/2022/015264 and PLG/2022/016016. K.C. acknowledges Czech Science Foundation grant no. 23-04746S and Project Quantum materials for applications in sustainable technologies (QM4ST), funded as project no. CZ.02.01.01/00/22_008/0004572 by P JAK, call Excellent Research by Ministry of Education, Youth and Sports of the Czech Republic.

Supporting Information

Supporting Information is available from the Elsevier Online Library or from the author.

References in Supporting Information

[40] The GE/IMI 7031 Varnish Is Obtained from Cambridge Magnetic Refrigeration, Cambridge, CB5 8HR, UK. Available online: https://www.cmr-direct.com/en/cmr-gevar-25ml?filter_name=ge%20varnis (accessed on 12 October 2022)., (n.d.).

[41] Nur Amanina Juniasari Tun Nur Iskandar, Yeap Guan Yeow, Nobuyuki Maeta, Masato M. Ito, Yoshiyuki Nakamura, Katarzyna Gas and Maciej Sawicki, Anisotropic and magnetic properties in non-metal and non-radical organic aggregates of tri-substituted phenyl derivatives, New J. Chem., 44, 210 (2020). DOI: 10.1039/C9NJ02730K

[42] M. Świątkowski, S. Lanka, A. Czylkowska, K. Gas, M. Sawicki, Structural, Spectroscopic, Thermal, and Magnetic Properties of a New Dinuclear Copper Coordination Compound with Tiglic Acid, Materials, 14, 2148 (2021). https://doi.org/10.3390/ma14092148

[43] B. Rogalewicz, A. Climova, E. Pivovarova, J. Sukiennik, K. Czarnecka, P. Szymański, M. Szczesio, K. Gas, M. Sawicki, M. Pitucha, and A. Czylkowska, Antitumor Activity and Physicochemical Properties of New Thiosemicarbazide Derivative and Its Co(II), Ni(II), Cu(II), Zn(II) and Cd(II) Complexes, Molecules 27, 2703 (2022); https://doi.org/10.3390/molecules27092703

[44] Quantum Design Application Note 1014-201, “Reciprocating Sample Option (RSO) – Theory of Operation and Measurement Modes,” Quantum Design Inc., San Diego, CA.

[65] W. Pacuski, P. Kossacki, D. Ferrand, A. Golnik, J. Cibert, M. Wegscheider, A. Navarro-Quezada, A. Bonanni, M. Kiecana, M. Sawicki, and T. Dietl, Observation of Strong-Coupling Effects in a Diluted Magnetic Semiconductor Ga1−xFexN\mathrm{Ga}_{1-x}\mathrm{Fe}_{x}\mathrm{N}, Phys. Rev. Lett. 100, 037204 (2008).

[68] A. Navarro-Quezada, K. Gas, T. Truglas, V. Bauernfeind, M. Matzer, D. Kreil, A. Ney, H. Groiss, M. Sawicki, and A. Bonanni, Out-of-Plane Magnetic Anisotropy in Ordered Ensembles of FeyN\mathrm{Fe}_{y}\mathrm{N} Nanocrystals Embedded in GaN, Materials 13, 3294 (2020).

[69] K. Gas, A. Królicka, K. Dybko, P. Nowicki, Z. Khosravizadeh, T. Story, and M. Sawicki, Magnetic constitution of topologically trivial thermoelectric PbTe:Cr\mathrm{PbTe:Cr}, Journal of Magnetism and Magnetic Materials 537, 168154 (2021).

[70] K. Gas, J. Sadowski, and M. Sawicki, Magnetic properties of wurtzite (Ga,Mn)As(\mathrm{Ga,Mn})\mathrm{As}, Journal of Magnetism and Magnetic Materials 533, 168012 (2021).

[71] K. Gas and M. Sawicki, Reliable Magnetometry for Antiferromagnets and Thin Films: Correcting Substrate Artifacts in Mn3Sn/MgO\mathrm{Mn}_{3}\mathrm{Sn/MgO} Systems, Phys. Rev. Appl., 25, 014012 (2026).

Supporting information

  • corresponding author – Małgorzata Wierzbowska

e-mail: [email protected], Phone: +48 22 6325010, Fax: +48 22 6324218

Illumination setup for SQUID magnetometry

To enable magnetization measurements under illumination, an alternative sample-mounting approach was used. This configuration also allowed us to extend the measurement temperature range up to 400 K, since it does not involve thermoplastic straws, which soften above approximately 340 K. Several milligrams of Cr2AlC\mathrm{Cr}_2\mathrm{AlC} powder were deposited onto a silicon platelet with dimensions of approximately 4×5×0.2 mm34 \times5 \times0.2\ \mathrm{mm}^3 and immobilized using highly diluted GE varnish [1], which has a negligible magnetic contribution. The complete specimen, consisting of the Si platelet with attached Cr2AlC\mathrm{Cr}_2\mathrm{AlC} powder, was then fixed with the same GE varnish to a silicon stick, approximately 8 inches long and 2 mm wide, which is the standard sample holder used in our MPMS setup [2]. This mounting configuration provides good thermal and mechanical stability [3, 4, 5], while allowing direct optical access to the powder surface.

For illumination-dependent measurements, a red LED was mounted at the upper end of the Si-stick holder, approximately 7 cm above the Cr2AlC\mathrm{Cr}_2\mathrm{AlC} powder, as shown in Figure S1. The emission wavelength of the diode was about 610 nm at 4 K. The LED was powered through two thin Cu wires connected to an external current source. The wires were routed to the laboratory environment through a custom-modified vacuum-tight electrical feedthrough integrated into the RSO head of the magnetometer.

Photograph of the illumination-compatible SQUID magnetometry setup

Figure S1. Photograph of the illumination-compatible SQUID magnetometry setup. The Cr2AlC\mathrm{Cr}_2\mathrm{AlC} powder was immobilized on a Si platelet attached to the Si-stick sample holder. A red LED was mounted above the sample and connected by thin Cu wires routed to the custom vacuum-tight feedthrough integrated into the magnetometer RSO-transport head.

To minimize the risk of insulation damage during reciprocating motion in the RSO mode, in particular possible shearing or abrasion of the wire enamel, the MaxSlope variant of the RSO mode was used for illuminated measurements [6]. In this mode, the sample travel distance is reduced from the standard 4 cm to 0.5 cm. A comparative test confirmed that magnetic moment values obtained in the standard full-scan RSO mode and in the MaxSlope mode agree within the experimental uncertainty.

The LED was typically operated at a current of approximately 1.5 mA. This was the highest current used in the experiment and was selected as a compromise between sufficient optical intensity at cryogenic temperatures and limited heating of the sample environment. The final illumination test, which also provides an estimate of the magnitude of LED-induced heating, is shown in Figure S2.

Temperature dependence of the magnetic moment of Cr₂AlC

Figure S2. Temperature dependence of the magnetic moment of Cr2_2AlC measured at H=10H = 10 kOe with the red LED switched on and off. The small displacement of the LED-on trace with respect to the LED-off reference is largest at low temperature, where dm/dTdm/dT is steepest, and is consistent with minor illumination-induced heating. Within the experimental sensitivity, the data do not indicate an intrinsic light-induced magnetic contribution beyond this heating effect.

The LED-on trace, measured on cooling, is shifted with respect to the LED-off reference measured on warming. Although this appears as a downward shift of the magnetic moment, the effect is more naturally interpreted as a small shift of the illuminated data toward lower nominal temperatures. Under illumination, the sample requires additional cooling power from the environment to compensate for the heat generated by the incoming radiation. Owing to the steep slope of m(T)m(T) in the liquid-helium temperature range, caused by the Curie-like contribution (part S3), the Cr2_2AlC sample effectively acts as a sensitive thermometer. The observed displacement can be reproduced by a small temperature offset of about 0.3 K at 2 K and less than 0.05 K at 5 K.

This temperature offset remained sufficiently small for testing possible optomagnetic effects. However, within the experimental sensitivity, no additional light-induced magnetic contribution was detected; the only observable outcome of illumination was the small, reversible, heating effect described above.

[1] The GE/IMI 7031 Varnish Is Obtained from Cambridge Magnetic Refrigeration, Cambridge, CB5 8HR, UK. Available online: https://www.cmr-direct.com/en/cmr-gevar-25ml?filter_name=ge%20varnis (accessed on 12 October 2022)., (n.d.).

[2] M. Sawicki, W. Stefanowicz, and A. Ney, Sensitive SQUID magnetometry for studying nanomagnetism, Semicond. Sci. Technol. 26, 064006 (2011).

[3] Nur Amanina Juniasari Tun Nur Iskandar, Yeap Guan Yeow, Nobuyuki Maeta, Masato M. Ito, Yoshiyuki Nakamura, Katarzyna Gas and Maciej Sawicki, Anisotropic and magnetic properties in non-metal and non-radical organic aggregates of tri-substituted phenyl derivatives, New J. Chem., 44, 210 (2020). DOI: 10.1039/C9NJ02730K

Magnetic phases obtained from the DFT and their relative total energies

Definitions of magnetic moments via the spin polarized electronic densities ρ↑(r)\rho^{\uparrow}(\mathbf{r}) and ρ↓(r)\rho^{\downarrow}(\mathbf{r}).

Mtot−total magnetic moment−∫ρ↑(r) dr−∫ρ↓(r) dr.M_{\mathrm{tot}} - \text{total magnetic moment} - \int\rho^{\uparrow}(\mathbf{r})\,\mathrm{d}r - \int\rho^{\downarrow}(\mathbf{r})\,\mathrm{d}r.
Mabs−absolute magnetic moment−is defined as:∫∣ρ↑(r)−ρ↓(r)∣ dr.M_{\mathrm{abs}} - \text{absolute magnetic moment} - \text{is defined as:} \quad\int\left|\rho^{\uparrow}(\mathbf{r})-\rho^{\downarrow}(\mathbf{r})\right|\,\mathrm{d}r.

Table S1. Magnetic phases of Cr2AlC\mathrm{Cr}_{2}\mathrm{AlC}. Total energies, ΔE\Delta E in meV, with respect to the paramagnetic state, total and absolute magnetic moments in in the cell (per 4 Cr atoms), MtotM_{\mathrm{tot}} and MabsM_{\mathrm{abs}} in μB\mu_{\mathrm{B}}, and relaxed lattice parameters, aa and cc in Å, obtained from the DFT with and without the spin-orbit coupling (SOC) employing the Perdew-Burke-Ernzerhof (PBE) or Perdew-Zunger (PZ) exchange-correlation functionals. Abreviations: PM – paramagnetic, AF – antiferromagnetic, FM – ferromagnetic phase. Experimental lattice vectors are a=2.910a=2.910 Å and c=13.097c=13.097 Å.

Quantification of low temperature paramagnetism

To probe the origin of the low-temperature paramagnetic, PM, component in magnetization of Cr2_2AlC, MPMM_{\mathrm{PM}}, and to determine its magnitude, we apply differential Brillouin function analysis, DBFA [7, 8, 9, 10, 11]. This approach is particularly suitable when a (weak) PM signal must be extracted from a (dominant) magnetic background whose magnetic field, HH, dependence is unknown, but whose temperature, TT, dependence is, or can be regarded, negligible at very low temperatures, that is where PM shows very strong TT-dependence. The DBFA is especially effective in systems with coexisting diamagnetic, Pauli-like, and/or ferromagnetic/antiferromagnetic/blocked-superparamagnetic contributions.

Data and preprocessing. We measure isothermal magnetization loops M(H)M(H) as functions of the magnetic field, HH, at 2, 5, and 8 K (and a 300 K reference). To suppress the TT-independent background, each low-TT curve can be baseline-corrected by subtracting the M(H,300 K)M(H, 300\ \mathrm{K}) trace. A mild over-compensation seen in Figure S3 is inconsequential for DBFA because the analysis uses pairwise differences between two nearby low-TT curves, in which any residual TT-independent part cancels.

Magnetic isotherms and differential Brillouin function differences

Figure S3. (a) Magnetic isotherms M(H)M(H) at low temperatures (indicated in the panel). The hatched area mark ΔMDFBA(H)\Delta M_{\mathrm{DFBA}}(H), the differences between M(H)M(H) at 2 and 5 K and 5 and 8 K. (b) The same differences re-plotted on the same coordinate frame (bullets) with an equivalent difference between Brillouin functions ΔMteo(H)\Delta M_{\mathrm{teo}}(H) calculated for spin S=3/2S = 3/2 (solid lines of corresponding hues). The matching factor between ΔMDFBA(H)\Delta M_{\mathrm{DFBA}}(H) and ΔMteo(H)\Delta M_{\mathrm{teo}}(H), nPMn_{\mathrm{PM}}, yields the concentration of paramagnetic spins in the sample.

The DBFA relies on the key observation that, at sufficiently low temperatures, the temperature dependence of non-paramagnetic contributions becomes negligible, whereas the magnetization of localized paramagnetic centers retains a strong temperature variability. Consequently, by subtracting isothermal magnetization curves measured at two nearby temperatures, the paramagnetic component can be isolated as:

ΔMDFBA(H)=M(T1,H)−M(T2,H)≈MPM(T1,H)−MPM(T2,H),\Delta M_{\mathrm{DFBA}}(H) = M(T_1,H) - M(T_2,H) \approx M_{\mathrm{PM}}(T_1,H) - M_{\mathrm{PM}}(T_2,H),

where MPMM_{\mathrm{PM}} denotes the component brought about by the paramagnetic spins at two nearby temperatures T1T_1 and T2T_2, T1<T2T_1 < T_2.

These differential magnetization curves ΔMDFBA(H)\Delta M_{\mathrm{DFBA}}(H), [bullets in Figure S3] can then be modeled using the difference of Brillouin functions taken at the same pairs of temperatures.

ΔMteo(H)=gμBnSS[BS(T1,H)−BS(T2,H)],\Delta M_{\mathrm{teo}}(H) = g\mu_{\mathrm{B}}n_{\mathrm{S}}S[B_{\mathrm{S}}(T_1,H)-B_{\mathrm{S}}(T_2,H)],

where gg is the Landé factor (taken here as g=2g = 2, μB\mu_{\mathrm{B}} is the Bohr magneton, nSn_{\mathrm{S}} is the concentration of spins, and BSB_{\mathrm{S}} is the Brillouin function defined as:

BS(x)=2S+12Scoth⁡(2S+12Sx)−12Scoth⁡(12Sx),x=SgμBHkBT,B_{\mathrm{S}}(x) = \frac{2S+1}{2S}\coth\left(\frac{2S+1}{2S}x\right)-\frac{1}{2S}\coth\left(\frac{1}{2S}x\right),\quad x = S\frac{g\mu_{\mathrm{B}}H}{k_{\mathrm{B}}T},

kBk_{\mathrm{B}} is the Boltzmann constant.

Importantly, the ΔMteo(H)\Delta M_{\mathrm{teo}}(H), the difference between two Brillouin functions taken at nearby temperatures produces a characteristic maximum, the position of which – for a given differences of temperatures – is highly sensitive to the spin quantum number SS. This makes the differential method exceptionally robust in determining the spin of the magnetic centers, even when the absolute PM signal is weak.

Fitting relevant ΔMteo(H)\Delta M_{\mathrm{teo}}(H) to ΔMDFBA(H)\Delta M_{\mathrm{DFBA}}(H) [the differences between M(H)M(H) taken here at 2 and 5 K and 5 and 8 K – these differences are marked as the hatched areas in both panels of Figure S3] yields S≈1.45S \approx1.45–1.551.55, indicating that the dominant spin component responsible for the low temperature paramagnetism comes from S=3/2S = 3/2 spins. Final fits, thick solid lines in Figure S3, performed with fixed S=3/2S = 3/2 provide a very good agreement with experimental data, yielding nS≃1.5×1018n_{\mathrm{S}} \simeq1.5 \times10^{18} spins per gram of Cr2_2AlC, and so a very low fraction of paramagnetic spins f≈0.00018f \approx0.00018 (~0.02%).

The parameters obtained in this way for the PM component of Cr2_2AlC reproduce the low-TT increase of MM, MPMM_{\mathrm{PM}}, very accurately. The compensated magnetic susceptibility curve, χ(T)=H−1[Mexp(T)−MPM(T)]\chi(T) = H^{-1}[M_{\mathrm{exp}}(T) - M_{\mathrm{PM}}(T)] (the blue symbols in Figure S4), indeed flattens out at low temperatures down to about 7 - 8 K. Below this temperature, a small deviation remains. It is most likely due to an additional, less abundant spin contribution, which also accounts for the residual uncertainty in SS. Nevertheless, the DBFA-based compensation enables a reliable analysis of Cr-Cr dimerization down to 8–10 K as presented in the main text.

Effectiveness of the removal of the paramagnetic component from temperature dependent data

Figure S4. Effectiveness of the removal of the paramagnetic component from temperature dependent data basing on the differential Brillouin function analysis.

Band structure calculated with the DFT

Absorption spectra obtained with the ai-BSE

0.211303310.16561547414361U D0.242
0.211303310.16561547414314U D0.268
0.211303310.16561547424329U-0.079
0.211303310.16561547424364D0.003
0.211303310.16561547454623U D0.001
0.279091660.19161962
0.279097170.20311963414336U D-0.262
0.280360430.22991975434524U D-0.234
0.280365410.13961976
0.281108050.21571984
0.338127380.11492418414216U0.127
0.338132110.13492419414217U0.127
0.339605930.36852458414218U0.135
0.340894730.24522491414262U0.130
0.340894730.24522491414335U-0.238
0.340894730.24522491414366U-0.208
0.340894730.24522491434440U D0.189
0.340894730.2452249143469U D-0.043
0.367657160.23022823424358U D-0.007
0.367657160.23022823424369D0.004
0.367657160.23022823434539U D-0.341
0.379154650.14012971414333U-0.020
0.379159180.12682972414334D0.052
0.393880550.20723218414317U D0.140
0.397389230.11453291414332U D0.006
0.397389230.11453291414362U D0.154
0.397389230.11453291414365U D0.016
0.397389230.11453291434442D0.001
0.412659440.13413514414331U0.021
0.412880360.18703517424418U D-0.225
0.412883520.22193518434531U D0.009
0.413281470.32093535434532U D-0.027
0.414441530.10213590434533U D-0.042
0.419322550.32743650434538U D-0.237
0.419844270.21633658434565U D-0.078
0.424490720.21743718414347D0.047
0.425247880.17983732434542U D0.037
0.447821350.14413922434541U D0.340
0.449143230.15493948434567U D0.222
0.449143230.15493948454639U D-0.215
0.497532700.19044508
0.497536150.20234509424431U D0.010
0.497604460.17724511434448U0.156
0.497605950.17914512
0.497791080.40114520
0.507837120.20004725424332D0.007
0.507839740.15844726424432U-0.032

Table 31.

ExE_x (eV)ffNo.bvalb_{\mathrm{val}}bcondb_{\mathrm{cond}}kkspinΔM\Delta M
0.507995610.15964732424453U D-0.064
0.507995610.15964732434465U D-0.044
0.507995610.15964732434469U D-0.140
0.616525350.14605743414420D0.002
0.616525350.14605743424522D0.008
0.616525350.14605743424523D0.007
0.616525350.14605743424537U D-0.153
0.628331840.18735839424440U D0.373
0.628696680.27615846424440U D0.373
0.653604510.11146091424447D0.052
0.653604510.11146091424525U D-0.425
0.682628100.17226536424441U D0.345
0.682628100.17226536424461U D0.038
0.682628100.17226536424467U D0.304
0.682628100.17226536434414D0.002
ExE_x (eV)ffNo.bvalb_{\mathrm{val}}bcondb_{\mathrm{cond}}kkspinΔM\Delta M
Electric field vector [0,0,1]
0.009976200.20711844459U D0.008
0.035516161.0000236424336U D-0.038
0.106668420.9232701454624U D0.035
0.106674580.3588703454624U D0.035
0.128273280.1003849424335U0.006
0.128273280.1003849424366D0.003
0.136079010.2495991424333U D0.046
0.136079010.2495991424346U D0.063
0.136079010.2495991444538U D-0.164
0.153610830.64291123414261U0.254
0.165693420.24901195424347U D0.242
0.165693420.2490119543454U-0.089
0.165693420.24901195444539D0.085
0.165693420.2490119544467D0.017
0.177033960.1202123343465U D-0.063
0.177033960.12021233434658U D-0.050
0.177033960.12021233444526U-0.030
0.178495230.50711263444526U D-0.077
0.179174510.11511277444563U D-0.079
0.204912040.56621412434439U D-0.210
0.215718170.10041589444527U D-0.105
0.216447770.22351603424345U D0.319
0.279916080.11471987434524U D-0.234

Table 32.

0.335884210.56192420414216D0.001
414217U D0.128
414262U D0.130
414335U D-0.177
414366U D-0.208
434440D-0.014
0.337653100.16162445414217U0.127
0.337814300.18552456414218U0.134
0.338673260.22002473424352U D0.429
43469U D-0.043
0.369269820.10902903434443U D0.228
0.386769530.26533110434624U D-0.199
0.398967980.1760337843458D-0.053
434517U-0.235
434559D0.020
434562U-0.276
0.432842080.26543824424536U D0.445
0.486713350.24834427434450U D0.083
43468U D-0.115
434659U D-0.101
0.497067510.10474547434423U D-0.223
434527U D-0.357
434648U D0.160
444626U D-0.118
444663U D-0.143
0.532099250.11535101434526U D-0.307
434563U D-0.383
0.638248800.19185938414419D0.003
43467U D-0.235
0.722563210.14007169434612U D-0.186
0.723003030.23587179434617U D-0.635
434627U D-0.262
434662U-0.725
424413U-0.373
424414U D-0.383
424461U-0.446
0.813465480.2149918841453D0.055
414532U-0.100
414565U-0.128
41463D0.035
434639U-0.575
0.826992690.29549467434611U D-0.351
434660U-0.340
0.890280010.165110594414414D-0.001
0.890476290.125310602414461D0.039
42467D0.009

Table 2.

434642D-0.068
454724U D-0.015
0.935150090.151111291434638U D-0.457
0.935150090.151111291434664U-0.663
0.935150090.15111129144478U-0.143
0.935150090.15111129144479D0.033
0.935150090.151111291444759U-0.183
0.935150090.15111129144487U-0.215
0.935150090.15111129144488D0.091
0.935150090.151111291444859U D-0.107
0.935150090.151111291454722U D-0.071
1.024200080.147112867414614U-0.607
1.024200080.147112867424543U D0.474
1.024200080.14711286743471U-0.508
1.024200080.14711286743472U-0.514
1.024200080.14711286743481U D-0.592
1.024200080.14711286743482U-0.603
1.024200080.14711286744471U-0.514
1.024200080.14711286744472U-0.507
1.024200080.14711286744481U-0.598
1.024200080.14711286744482U-0.597
1.024200080.14711286744485D0.080
1.024200080.14711286744486U D-0.297
1.024200080.147112867444858D0.006
1.284712790.106015725424552U D0.412
1.361248730.130116698434835D0.015
1.361248730.130116698434866U D-0.473
1.374356630.185416851434841U D-0.267
1.374356630.185416851434867U D-0.255
1.407358410.103517147424640U D-0.084
1.407358410.103517147434868U-0.388
1.432070850.125717486414718U D0.095
1.460154530.156517779424711D0.039
1.460154530.156517779434755U0.182
1.460154530.156517779434760U-0.230
1.572896360.236918999414812U D-0.764
1.597965240.104719310414815U-0.696
1.606208560.193319347414732U D-0.254
1.606208560.193319347414765U D-0.269
1.606208560.193319347424827U D-0.454
1.607953910.104219393414728U D-0.494
1.607953910.104219393414765D0.121
1.790121080.16632133841486D0.119
1.790121080.166321338424852D0.149

Table 1 (PDF p. 34).

References

  1. [1]N. Fang, C. Wu, Y. Zhang, Z. Li, Z. Zhou, Perspectives: Light Control of Magnetism and Device Development, ACS Nano 18 (2024) 8600–8625, https://doi/10.1021/acsnano.3c13002.DOI
  2. [2]E. Beaurepaire, J.-C. Merle, A. Daunois, J.-Y. Bigot, Ultrafast Spin Dynamics in Ferromagnetic Nickel, Phys. Rev. Lett. 76 (1996) 4250–4253, https://doi.org/10.1103/PhysRevLett.76.4250.
  3. [3]A. Kirilyuk, A.V. Kimel, T. Rasing, Ultrafast optical manipulation of magnetic order, Rev. Mod. Phys. 82 (2010) 2731–2784, https://doi.org/10.1103/RevModPhys.82.2731.
  4. [4]K. Carva, M. Battiato, P.M. Oppeneer, Ab Initio Investigation of the Elliott-Yafet Electron-Phonon Mechanism in Laser-Induced Ultrafast Demagnetization, Phys. Rev. Lett. 107 (2011) 207201, https://doi.org/10.1103/PhysRevLett.107.207201.
  5. [5]S.R. Tauchert, M. Volkov, D. Ehberger, D. Kazenwadel, M. Evers, H. Lange, A. Donges, A. Book, W. Kreuzpaintner, U. Nowak, P. Baum, Polarized phonons carry angular momentum in ultrafast demagnetization, Nature 602 (2022) 73–77, https://doi.org/10.1038/s41586-021-04306-4.
  6. [6]V. Unikandanunni, R. Medapalli, E.E. Fullerton, K. Carva, P.M. Oppeneer, S. Bonetti, Anisotropic ultrafast spin dynamics in epitaxial cobalt, Applied Physics Letters 118 (2021) 232404, https://doi.org/10.1063/5.0049692.
  7. [7]M. Haag, C. Illg, M. Fähnle, Role of electron-magnon scatterings in ultrafast demagnetization, Phys. Rev. B 90 (2014) 014417, https://doi.org/10.1103/PhysRevB.90.014417.
  8. [8]M. Weißelhofer, P. M. Oppeneer, Ultrafast Demagnetization Through Femtosecond Generation of Non-Thermal Magnons, Adv. Phys. Res. (2024) 2300103, https://doi.org/10.1002/apxr.202300103.
  9. [9]M. Battiato, K. Carva, P. M. Oppeneer, Superdiffusive Spin Transport as a Mechanism of Ultrafast Demagnetization, Phys. Rev. Lett. 105 (2010) 027203, https://doi.org/10.1103/PhysRevLett.105.027203.
  10. [10]M. Hofherr et al., Ultrafast optically induced spin transfer in ferromagnetic alloys, Sci. Adv. 6 (2020) eaay8717, https://doi.org/10.1126/sciadv.aay8717.
  11. [11]K. Carva, P. Baláž, and I. Radu, in Handbook of Magnetic Materials, Vol. 26, edited by E. Brück (Elsevier, 2017), pp. 291–463.
  12. [12]J.K. Dewhurst, S. Shallcross, P. Elliott, S. Eisebitt, C. v. Korff Schmisинг, C. v. Korff, S. Sharma, Angular momentum redistribution in laser-induced demagnetization, Phys. Rev. B 104 (2021) 054438, https://doi.org/10.1103/PhysRevB.104.054438.
  13. [13]C. von Korff Schmising, S. Jana, O. Zülich, D. Sommer, S. Eisebitt, Direct versus indirect excitation of ultrafast magnetization dynamics in FeNi alloys, Physical Review Research 6 (2024) 013270, https://doi.org/10.1103/PhysRevResearch.6.013270.
  14. [14]M. S. Mrudul, P. M. Oppeneer, Ab initio investigation of laser-induced ultrafast demagnetization of FePt: Intensity dependence and importance of electron coherence, Phys. Rev. B 109 (2024) 144418, https://doi.org/10.1103/PhysRevB.109.144418.
  15. [15]T. Jungwirth, X. Marti, P. Wadley, J. Wunderlich, Antiferromagnetic spintronics. Nature Nanotech 11 (2016) 231–241, https://doi.org/10.1038/nnano.2016.18.
  16. [16]J. H. Mentink, J. Hellsvik, D.V. Afanasiev, B.A. Ivanov, A. Kirilyuk, A.V. Kimel, O. Eriksson, M.I. Katsnelson, Th. Rasing, Ultrafast Spin Dynamics in Multisublattice Magnets, Phys. Rev. Lett. 108 (2012) 057202, https://doi.org/10.1103/PhysRevLett.108.057202.
  17. [17]S.-E. Lee, Y. W. Windsor, A. Fedorov, K. Kliemt, C. Krellner, C. Schüßler-Langeheine, N. Pontius, M. Wolf, U. Atxitia, D. V. Vyalikh, L. Rettig, Robust Magnetic Order Upon Ultrafast Excitation of an Antiferromagnet, Advanced Materials Interfaces 9 (2022) 2201340, https://doi.org/10.1002/admi.202201340.
  18. [18]Y. W. Windsor, A. Ernst, K. Kummer, K. Kliemt, Ch. Schüßler-Langeheine, N. Pontius, U. Staub, E. V. Chulkov, C. Krellner, D. V. Vyalikh, L. Rettig, Deterministic control of an antiferromagnetic spin arrangement using ultrafast optical excitation, Communications Physics 3 (2020) 139, https://doi.org/10.1038/s42005-020-00407-0.
  19. [19]D. Hamara, M. Strungaru, J.R. Massey, et al., Ultra-high spin emission from antiferromagnetic FeRh, Nature Communications 15 (2024) 4958, https://doi.org/10.1038/s41467-024-48795-z.
  20. [20]Z. Kašpar, M. Surýnek, J. Zubáč, F. Krizek, V. Novák, R.P. Campion, M.S. Wörнle, P. Gambardella, X. Marti, P. Němec, K.W. Edmonds, S. Reimers, O.J. Amin, F. Maccherოზzi, S.S. Dhesi, P. Wadley, J. Wunderlich, K. Olejník, T. Jungwirth, Quenching of an antiferromagnet into high resistivity states using electrical or ultrashort optical pulses, Nature Electronics 4 (2021) 30–37, https://doi.org/10.1038/s41928-020-00506-4.
  21. [21]F. Freimuth, S. Blügel, and Y. Mokrousov, Laser-induced torques in metallic antiferromagnets, Phys. Rev. B 103 (2021) 174429, https://doi.org/10.1103/PhysRevB.103.174429.
  22. [22]T. Dannegger, M. Beritta, K. Carva, S. Selzer, U. Ritzmann, P.M. Oppeneer, U. Nowak, Ultrafast coherent all-optical switching of an antiferromagnet with the inverse Faraday effect, Physical Review B 104 (2021) L060413, https://doi.org/10.1103/PhysRevB.104.L060413.
  23. [23]N. Kubitza, C. Büchner, J. Sinclair, R. M. Snyder, and C. S. Birkel, Extending the Chemistry of Layered Solids and Nanosheets: Chemistry and Structure of MAX Phases, MAB Phases and Mxenes, ChemPlusChem 88 (2023) e202300214, https://doi.org/10.1002/cplu.202300214.
  24. [24]Z. Fu, N.Wang, D. Legut, C. Si, Q. Zhang, S. Du, T.C. Germann, J.S. Francisco, R. Zhang, Rational Design of Flexible Two-Dimensional MXenes with Multiple Functionalities, Chem Rev. 119 (2019) 11980–12031, https://doi.org/10.1021/acs.chemrev.9b00348.
  25. [25]M. Khazaei, A. Ranjbar, M. Arai, T. Sasaki, S. Yunoki, Electronic properties and applications of MXenes: a theoretical review, Journal of Materials Chemistry C 5 (2017) 2488, https://doi.org/10.1039/C7TC00140A
  26. [26]X. Lin, W. Yang, K. L. Wang, and W. Zhao, Two-dimensional spintronics for low-power electronics, Nature Electronics 2 (2019) 274–283, https://doi.org/10.1038/s41928-019-0273-7.
  27. [27]A. Hirohata, K. Yamadab, Y. Nakatanić, I.-L. Prejbeanuḍ, B. Diényḍ, P. Pirroee, B. Hillebrands, Review on spintronics: Principles and device applications, Journal of Magnetism and Magnetic Materials 509 (2020) 166711, https://doi.org/10.1016/j.jmmm.2020.166711.
  28. [28]M. Gibertini, M. Koperski, A.F. Morpurgo, K.S. Novoselov, Magnetic 2D materials and heterostructures, Nat. Nanotechnol. 14 (2019) 408–419, https://doi.org/10.1038/s41565-019-0438-6.
  29. [29]K. Hantanasirisakul, B. Anasori, S. Nemšak, J.L. Hart, J. Wu, Y. Yang, R.V. Chopdekar, P. Shafer, A.F. May, E.J. Moon, J. Zhou, Q. Zhang, M.L. Taheri, S.J. May, Y. Gogotsi, Evidence of a magnetic transition in atomically thin Cr2TiC2Tx Mxene, Nanoscale Horizons 5 (2020) 1557–1565, https://doi.org/10.1039/D0NH00343C.
  30. [30]M. Imam, J. Fatheema, Q. Noor, M. Rani, M. Mumtaz, R.-K. Zheng, S.A. Khan, S. Rizwan, Co-existence of magnetic phases in two-dimensional Mxene, Materials Today Chemistry 16 (2020) 100271, https://doi.org/10.1016/j.mtchem.2020.100271.
  31. [31]M. Jaouen, P. Chartier, T. Cabioch, V. Mauchamp, G. André, M. Viret, Invar Like Behavior of the Cr2AlC MAX Phase at Low Temperature, J. Am. Ceram. Soc., 96: 3872–3876, https://doi.org/10.1111/jace.12635.
  32. [32]M. Dahlqvist, B. Alling, I. A. Abrikosov, J. Rosen, Phys. Rev. B 84 (2011) 220403, https://doi.org/10.1103/PhysRevB.84.220403.
  33. [33]K.V. Sobolev, K.K. Kolincio, A. Emelyanov, A. Mielewczyk-Gryń, M. Gazda, M. Roman, A. Pazniak, V. Rodionov, Evolution of magnetic and transport properties in (Cr1−xMnx)2AlC MAX-phase synthesized by arc melting technique, Journal of Magnetism and Magnetic Materials 493 (2020) 165642, https://doi.org/10.1016/j.jmmm.2019.165642.
  34. [34]K. Sobolev, H. Pazniak, M. Farle, V. Rodionova, and U. Wiedwald, Synthesis, phase purification and magnetic characterization of the (Cr1-x,Mnx)2AlC MAX-phase, Journal of Materials Chemistry C 9 (2021) 16516, https://doi.org/10.1039/d1tc03092b.
  35. [35]J. Gonzalez-Julian, S. Onrubia, M. Bram, O. Guillon, Effect of sintering method on the microstructure of pure Cr2AlC MAX phase ceramics, J. Ceram. Soc. Jap. 124 (2016) 415–420, https://doi.org/10.2109/jcersj2.15263.
  36. [36]C. Azina, M. Poll, D.M. Holzapfel, E. Tailleur, A. Zuber, S. Dubois, P. Eklund, J. Gonzalez-Julian, Microstructural and compositional design of Cr2AlC MAX phases and their impact on oxidation resistance, J. Eur. Ceram. Soc. 44 (2024) 4895–4904, https://doi.org/10.1016/j.jeurceramsoc.2024.02.037.
  37. [37]K. Sierakowski, R. Jakiela, B. Lucznik, P. Kwiatkowski, M. Iwinska, M. Turek, H. Sakurai, T. Kachi, M. Bockowski, High Pressure Processing of Ion Implanted GaN, Electronics 9 (2020) 1380, https://doi.org/10.3390/electronics9091380.
  38. [38]M. Sawicki, W. Stefanowicz, and A. Ney, Sensitive SQUID magnetometry for studying nanomagnetism, Semicond. Sci. Technol. 26, 064006 (2011).DOI
  39. [39]K. Gas and M. Sawicki, In Situ Compensation Method for Precise Integral SQUID Magnetometry of Miniscule Biological, Chemical, and Powder Specimens Requiring the Use of Capsules. Materials 15, 2 (2022).DOI
  40. [40]The GE/IMI 7031 Varnish Is Obtained from Cambridge Magnetic Refrigeration, Cambridge, CB5 8HR, UK. Available online: https://www.cmr-direct.com/en/cmr-gevar-25ml?filter_name=ge%20varnis (accessed on 12 October 2022)., (n.d.).
  41. [41]Nur Amanina Juniasari Tun Nur Iskandar, Yeap Guan Yeow, Nobuyuki Maeta, Masato M. Ito, Yoshiyuki Nakamura, Katarzyna Gas and Maciej Sawicki, Anisotropic and magnetic properties in non-metal and non-radical organic aggregates of tri-substituted phenyl derivatives, New J. Chem., 44, 210 (2020). DOI: 10.1039/C9NJ02730K
  42. [42]M. Świątkowski, S. Lanka, A. Czylkowska, K. Gas, M. Sawicki, Structural, Spectroscopic, Thermal, and Magnetic Properties of a New Dinuclear Copper Coordination Compound with Tiglic Acid, Materials, 14, 2148 (2021). https://doi.org/10.3390/ma14092148
  43. [43]B. Rogalewicz, A. Climova, E. Pivovarova, J. Sukiennik, K. Czarnecka, P. Szymański, M. Szczesio, K. Gas, M. Sawicki, M. Pitucha, and A. Czylkowska, Antitumor Activity and Physicochemical Properties of New Thiosemicarbazide Derivative and Its Co(II), Ni(II), Cu(II), Zn(II) and Cd(II) Complexes, Molecules 27, 2703 (2022); https://doi.org/10.3390/molecules27092703
  44. [44]Quantum Design Application Note 1014-201, “Reciprocating Sample Option (RSO) – Theory of Operation and Measurement Modes,” Quantum Design Inc., San Diego, CA.
  45. [45]K. Marumoto, T. Fujimori, M. Ito, T. Mori, Advanced Energy Materials 2 (2012) 591–597, https://doi.org/10.1002/aenm.201100774.
  46. [46]T. Nagamori, K. Marumoto, Direct Observation of Hole Accumulation in Polymer Solar Cells During Device Operation using Light-Induced Electron Spin Resonance, Advanced Materials 25 (2013) 2362-2367, https://doi.org/10.1002/adma.201204015.
  47. [47]P. Hohenberg, W. Kohn, Inhomogeneous Electron Gas, Phys. Rev. B 136 (1964) B864-B871, https://doi.org/10.1103/PhysRev.136.B864.
  48. [48]W. Kohn, L.J. Sham, Self-Consistent Equations Including Exchange and Correlation Effects, Phys. Rev. B 140 (1965) A1133–A1138, https://doi.org/10.1103/PhysRev.140.A1133.
  49. [49]P. Giannozzi, S. Baroni, N. Bonini, M. Calandra, R. Car, C. Cavazzoni, D. Ceresoli, G.L. Chiarotti, M. Cococcioni, I. Dabo, et al., Quantum espresso: a modular and open-source software project for quantum simulations of materials, J. Phys.: Condens. Matter. 21 (2009) 395502, https://doi.org/10.1088/0953-8984/21/39/395502.
  50. [50]J.P. Perdew, K. Burke, M. Ernzerhof, Generalized gradient approximation made simple, Phys. Rev. Lett. 77 (1996) 3865–3868, https://doi.org/10.1103/PhysRevLett.77.3865.
  51. [51]H.J. Monkhorst, J.D. Pack, Special Points for Brillouin-Zone Integrations, Physical Review B, 13 (1976) 5188-5192, http://dx.doi.org/10.1103/PhysRevB.13.5188.
  52. [52]E.E. Salpeter, H.A. Bethe, A relativistic equation for bound-state problems. Phys. Rev. 84 (1951) 1232–1242, https://doi.org/10.1103/PhysRev.84.1232.
  53. [53]A. Marini, C. Hogan, M. Grüning, D. Varsano, Yambo: an ab initio tool for excited state calculations, Comput. Phys. Commun. 180 (2009) 1392–1403, https://doi.org/10.1016/j.cpc.2009.02.003.
  54. [54]D. Sangalli, A. Ferretti, H. Miranda, C. Attaccalite, I. Marri, E. Cannuccia, P. Melo, M. Marsili, F. Paleari, A. Marrazzo, Many-body perturbation theory calculations using the yambo code, J. Phys. Cond. Matter. 31 (2019) 325902, https://doi.org/10.1088/1361-648X/ab15d0.
  55. [55]J.C. Taylor, Tamm-Dancoff Method, Phys. Rev. 95 (1954) 1313–1317, https://doi.org/10.1103/PhysRev.95.1313.
  56. [56]I. Souza, N. Marzari, D. Vanderbilt, Maximally localized Wannier functions for entangled energy bands, Phys. Rev. B 65 (2001) 035109, https://doi.org/10.1103/PhysRevB.65.035109.
  57. [57]N. Marzari, A.A. Mostofi, J.R. Yates, I. Souza, D. Vanderbilt, Maximally localized Wannier functions: Theory and applications, Rev. Mod. Phys. 84 (2012) 1419, https://doi.org/10.1103/RevModPhys.84.1419
  58. [58]G. Pizzi, et al. Wannier90 as a community code: new features and applications. J. Phys. Cond. Mater. 32 (2020) 165902, https://doi.org/10.1088/1361-648X/ab51ff.
  59. [59]W. Jeitschko, H. Nowotny, Die Kristallstruktur von Ti₃SiC₂—ein neuer Komplexcarbid-Typ, Monatsh. Chem. 98 (1967) 329, https://doi.org/10.1007/BF00899949.
  60. [60]J. Yuan, S. Zhou, H. Wu, Z. Wang, Y. Zhang, G. Zhou, G. Ma, P. Ke, A. Wang, Ultrahigh strength-ductility of nanocrystalline Cr₂AlC coating under micropillar compression, Scipta Materialia, 235 (2023) 115594, https://doi.org/10.1016/j.scriptamat.2023.115594.
  61. [61]Z. Wang, G. Ma, L. Liu, L. Wang, P. Ke, Q. Xue, A. Wang, High-performance Cr₂AlC MAX phase coatings: Oxidation mechanisms in the 900–1100°C temperature range, Corrosion Science, 167 (2020) 108492, https://doi.org/10.1016/j.corsci.2020.108492.
  62. [62]P. Sharma, O.P. Pandey, Thermal kinetics involved during the solid-state synthesis of Cr₂AlC MAX phase. J Therm Anal Calorim,143 (2021) 3997–4008, https://doi.org/10.1007/s10973-020-09390-8.
  63. [63]Gordon A. Bain and John F. Berry, Diamagnetic Corrections and Pascal’s Constants, Journal of Chemical Education, 85 (2008) 532DOI
  64. [64]Zhongsheng Liu, Kenta Takao, Takeshi Waki, Yoshikazu Tabata and Hiroyuki Nakamura, Electron correlation in Pauli paramagnetic Cr₂AlC, Cr₂GaC and Cr₂GeC, 2017 J. Phys.: Conf. Ser. 868 012016; DOI 10.1088/1742-6596/868/1/012016DOI
  65. [65]W. Pacuski, P. Kossacki, D. Ferrand, A. Golnik, J. Cibert, M. Wegscheider, A. Navarro-Quezada, A. Bonanni, M. Kiećana, M. Sawicki, and T. Dietl, Observation of Strong-Coupling Effects in a Diluted Magnetic Semiconductor Ga₁₋ₓFeₓN, Phys. Rev. Lett. 100, 037204 (2008).pubmed.ncbi.nlm.nih.gov/18233033
  66. [66]Z. Liu, T. Waki, Y. Tabata, and H. Nakamura, Mn-doping-induced itinerant-electron ferromagnetism in Cr₂GeC, Phys. Rev. B 89 (2014) 054435.
  67. [67]Christin M. Hamm, Joshua D. Bocarsly, Gareth Seward, Ulrike I. Kramm and Christina S. Birkel, Non-conventional synthesis and magnetic properties of MAX phases (Cr/Mn)₂AlC and (Cr/Fe)₂AlC, J. Mater. Chem. C, 2017, 5, 5700; DOI: 10.1039/c7tc00112fDOI
  68. [68]A. Navarro-Quezada, K. Gas, T. Truglas, V. Bauernfeind, M. Matzer, D. Kreil, A. Ney, H. Groiss, M. Sawicki, and A. Bonanni, Out-of-Plane Magnetic Anisotropy in Ordered Ensembles of FeᵧN Nanocrystals Embedded in GaN, Materials 13, 3294 (2020).
  69. [69]K. Gas, A. Królicka, K. Dybko, P. Nowicki, Z. Khosravizadeh, T. Story, and M. Sawicki, Magnetic constitution of topologically trivial thermoelectric PbTe:Cr, Journal of Magnetism and Magnetic Materials 537, 168154 (2021).DOI
  70. [70]K. Gas, J. Sadowski, and M. Sawicki, Magnetic properties of wurtzite (Ga,Mn)As, Journal of Magnetism and Magnetic Materials 533, 168012 (2021).DOI
  71. [71]K. Gas and M. Sawicki, Reliable Magnetometry for Antiferromagnets and Thin Films: Correcting Substrate Artifacts in Mn₃Sn/MgO Systems, Phys. Rev. Appl., 25, 014012 (2026).DOI
  72. [72]Bleaney, B.; Bowers, K.D. Anomalous paramagnetism of copper acetate. Proc. R. Soc. Lond. Ser. A 1952, 214, 451–465.
  73. [73]C. J. O’Connor, Magnetochemistry-Advances in Theory and Experimentation, Progress in Inorganic Chemistry; Vol 29, Edited by Stephen J. Lippard, John Wiley & Sons, Inc. (1982).DOI
  74. [74]G. Frenking, Heretical thoughts about the present understanding and description of the chemical bond. Molecular Physics, 121 (9–10) (2022) https://doi.org/10.1080/00268976.2022.2110168

Paper details

vlnc:W_rbe57ypk
Version
v1 · latest
Published
Fresh — added to the Hub within the last 30 days
Added
License
CC BY 4.0
Usage

views · 0

downloads · 0

A view counts once per browser per day, a download each time the PDF is requested.

  • Physics and Astronomy

Not recorded for this paper

View statement
Looking for related papers…
Contents