betaFeedback

WorksPhysics and Astronomy

Anomalous Electrical Transport in the Kagome Magnet YbFe6_6Ge6_6

Abstract

Two-dimensional (2D) kagome metals offer a unique platform for exploring electron correlation phenomena derived from quantum many-body effects. Here, we report a combined study of electrical magnetotransport and neutron scattering on YbFe6_6Ge6_6, where the Fe moments in the 2D kagome layers exhibit an AA-type collinear antiferromagnetic order below TN≈500T_{\rm{N}} \approx 500 K. Interactions between the Fe ions in the layers and the localized Yb magnetic ions in between reorient the cc-axis aligned Fe moments to the kagome plane below TSR≈63T_{\rm{SR}} \approx 63 K. Our magnetotransport measurements show an intriguing anomalous Hall effect (AHE) that emerges in the spin-reorientated collinear state, accompanied by the closing of the spin anisotropy gap as revealed from inelastic neutron scattering. The gapless spin excitations and the Yb-Fe interaction are able to support a dynamic scalar spin chirality, which explains the observed AHE. Therefore, our study demonstrates spin fluctuations may provide an additional scattering channel for the conduction electrons and give rise to AHE even in a collinear antiferromagnet.

The Hall effect, discovered by Edwin Hall, is the potential difference across an electric conductor transverse to the current and to an externally applied magnetic field perpendicular to the current [1]. For conventional metals or semiconductors, the ordinary Hall effect (voltage) is linearly proportional to the applied magnetic field. The anomalous Hall effect (AHE), one of the most prominent phenomena of quantum transport in correlated electron materials, describes unconventional electron deflection other than the effect of external magnetic fields [2, 3, 4]. While the initial observation of AHE was made in ferromagnets (conventional AHE) [2], AHE can also occur in materials without net magnetization. The observation of AHE in antiferromagnets is of particular interest, where the interplay of itinerant electrons and spin texture (i.e., magnetic structure) gives rise to this unique transport property [5, 6, 7]. From the application perspective, antiferromagnetic (AFM) spintronic devices have advantages over ferromagnetic counterparts, such as the absence of stray fields and being robust to external magnetic field perturbation [8].

Therefore, a determination of the microscopic origin of the AHE in antiferromagnets has been attracting great interest. For example, it is well-known that a real-space Berry phase originating from a magnetic field-induced skyrmion lattice (non-coplanar spin texture) can produce an AHE termed “topological Hall effect” (THE) [9, 10, 11, 12, 13, 14]. The non-coplanar spin texture of a skyrmion has a non-zero scalar spin chirality (SSC) χijk=Si⋅(Sj×Sk)\chi_{ijk} = \mathbf{S}_i \cdot(\mathbf{S}_j \times\mathbf{S}_k), where Si\mathbf{S}_i, Sj\mathbf{S}_j, and Sk\mathbf{S}_k are three localized spins at sites ii, jj, and kk, that acts as a fictitious magnetic field to induce AHE [4]. The chiral spin texture of a magnetic skyrmion is often stabilized by the competition of Heisenberg and Dzyaloshinskii-Moriya interactions [9, 10, 11].

Going beyond the paradigm of the static spin effect, recent studies suggest that fluctuating spins can also contribute to the AHE by scattering the electrons, even in the spin-disordered state [15, 16, 17, 18]. Arranging spins in a triangular motif is considered to be a favorable condition [18], as spin fluctuations could be significantly promoted by the geometrical frustration. The kagome lattice, a two-dimensional (2D) network of corner-sharing triangles, is an ideal platform to realize this mechanism. Indeed, spin-fluctuation driven AHE/THE was recently observed in some kagome magnets, including AMn6_6Sn6_6 (AA = Y, Sc, and Er) [19, 20, 21, 22], B3_3Ru4_4Al12_{12} (BB = Nd and Gd) [23, 24], and HoAgGe [25]. In these materials, non-zero time-averaged SSC ⟨Si⋅(Sj×Sk)⟩\langle S_i \cdot(S_j \times S_k) \rangle is induced by spin fluctuations out of noncollinear magnetic structures or paramagnetic states. However, there is no direct evidence of such spin fluctuations, for example, by inelastic neutron scattering (INS) experiments, particularly in the temperature region where the AHE was detected. In addition, it is still unclear whether spin fluctuations from collinear AFM structures can have ⟨Si⋅(Sj×Sk)⟩≠0\langle S_i \cdot(S_j \times S_k) \rangle\ne0 and therefore AHE/THE.

Here we report the discovery of a spin-fluctuation driven AHE in the kagome lattice magnet YbFe6_6Ge6_6 with a collinear AFM structure [26, 27, 28, 29, 30]. Through a comprehensive study of magnetization, magnetotransport, and neutron diffraction on single crystals, we find that the AHE emerges in its spin-reorientated state below TSR≈63T_{\mathrm{SR}} \approx63 K, where the collinear Fe spins rotate from the cc-axis to the kagome plane. The combined space inversion and time-reversal (ITIT) symmetry of the magnetic structure rules out the static non-zero SSC being the origin of the AHE [5, 6, 7]. Since our INS experiments reveal gapless low-energy spin excitations in the spin-reoriented state, the highly fluctuating Fe spins can contribute to a dynamic non-zero SSC by interacting with the Yb spins, which thereby induces the AHE [31].

The crystal structure of YbFe6_6Ge6_6 is shown in Figure 1(a), where the Fe ions form a 2D kagome lattice. YbFe6_6Ge6_6 belongs to the family of hexagonal RFe6_6Ge6_6 compounds (with RR = Sc, Yb, Lu, Mg, Ti, Zr, Hf, and Nb) [26, 28, 32, 33, 34]. Their structure is derived by inserting the RR ions into the B35 structure FeGe [35]. Despite the fact that they all have a Néel temperature well above room temperature, YbFe6_6Ge6_6 is the only member exhibiting a spontaneous spin reorientation (SR) transition [26, 28, 32, 33, 34]. Yb has been determined to be trivalent, yet its triangular lattice does not order at least above 0.4 K [27, 28, 36]. Thus the magnetism of YbFe6_6Ge6_6 is mainly given by the Fe kagome lattice, although there must also be Yb-Fe interactions at low temperatures.

Crystal structure, resistivity, magnetic susceptibility, and magnetization of YbFe6Ge6

Figure 1. (a) Crystal structure of YbFe6_6Ge6_6. Right inset shows the local structure of Yb and Fe, with one spin triad of Yb-Fe highlighted in yellow. (b) Temperature dependence of zero-field resistivity in the kagome plane. Inset shows its derivative with respect to temperature. (c) Temperature dependence of DC magnetic susceptibility under a field of 1 T parallel and perpendicular to the cc-axis. (d) Isothermal magnetizations along the a∗\mathbf{a}^{*} direction up to 9 T at selected temperatures. Inset shows the magnetizations up to 50 T at 4 K and 100 K.

The zero-field resistivity of YbFe6_6Ge6_6 along the kagome plane is presented in Figure 1(b), which shows a typical metallic behavior with a residual-resistivity ratio of ∼12\sim12. The derivative of the resistivity shows a small yet sharp peak around TSRT_{\mathrm{SR}}, indicating the change of magnetic structure. Figure 1(c) shows the DC magnetic susceptibility under a magnetic field of 1 T along and perpendicular to the cc-axis. The sudden susceptibility change around 63 K confirms the occurrence of the SR transition. These electrical and magnetic characteristics are consistent with an early report [28].

Next, we explore how external fields affect the magnetic and transport properties of YbFe6_6Ge6_6. Figure 1(d) presents the isothermal magnetization along the a∗\mathbf{a}^{*} direction at selected temperatures from 10 K to 100 K. Although the magnetization shows an overall linear dependence on the field, it is slightly nonlinear at low fields for T<TSRT < T_{\mathrm{SR}}. However, the magnitude of magnetization is quite small. Even at a magnetic field of 50 T, the moment size is only about 0.3 μB\mu_{\mathrm{B}}/Fe [inset of Figure 1(d)], which is much smaller than the full moment size of ∼\sim1.5 μB\mu_{\mathrm{B}}/Fe [26, 27, 29, 30, 36]. The contrast between T>TSRT > T_{\mathrm{SR}} and T<TSRT < T_{\mathrm{SR}} can be more clearly discerned in the magnetoresistance (MR) [Figure 2(a)], with MR=[ρxx(B)−ρxx(0)]/ρxx(0)\mathrm{MR} = [\rho_{xx}(B) - \rho_{xx}(0)]/\rho_{xx}(0). Here the magnetic field is also applied along the a∗\mathbf{a}^{*} direction. At 80 K, the MR has an approximately quadratic dependence on the field up to 12 T. When cooling below TSRT_{\mathrm{SR}}, it first increases rapidly at low field and then shows the approximately quadratic behavior at high fields. Similar MR behavior was observed in Fe3_3Sn2_2, which is typical of metallic magnets with an SR transition [37, 38].

Magnetoresistance, Hall resistivity, remnant Hall conductivity, and contour plot

Figure 2. (a) Magnetoresistance at selected temperatures under fields along the a∗a^* direction. The electric current is along the bb-axis. (b) Hall resistivity at selected temperatures under fields along the a∗a^* direction. Dashed curves in (a) and (b) are the fits with the two-band model [36]. (c) Remnant Hall conductivity (Δσxy\Delta\sigma_{xy}) after subtracting the ordinary Hall contribution. Inset shows the Hall measurement configuration. (d) Contour plot of Δσxy\Delta\sigma_{xy} for temperatures from 10 K to 80 K and magnetic fields from 0 T to 12 T.

Field dependence of the Hall resistivity is shown in Figure 2(b), where we find a drastic change of ρyx\rho_{yx} from 10 K to 80 K. In magnetic systems, the Hall resistivity can be decomposed into three parts: ρyx=ρyxO+ρyxA+Δρyx\rho_{yx} = \rho_{yx}^{O} + \rho_{yx}^{A} + \Delta\rho_{yx} [31, 39], where ρyxO\rho_{yx}^{O} is ordinary Hall resistivity, ρyxA\rho_{yx}^{A} is conventional anomalous Hall resistivity due to net magnetization (ρyxA∝M\rho_{yx}^{A} \propto M), and Δρyx\Delta\rho_{yx} is additional AHE contributions that cannot be included in the former two parts. For a magnetic system with localized moments, Δρyx\Delta\rho_{yx} usually comes from static and/or dynamic spin textures. In our case, MM is very small and shows barely temperature dependence [Figure 1(d)], which is in contrast to the temperature evolution of ρyx\rho_{yx} Figure 2(b). Therefore, ρyxA\rho_{yx}^{\mathrm{A}} is negligible, and we focus on the remaining two parts.

The nonlinear field dependence of MR and ρyx\rho_{yx} indicates a dominant multiband behavior. We use a two-band model to simultaneously fit the MR and ρyx\rho_{yx} [38, 40, 41]. Although the data at high fields can be well described by the two-band model, evident deviation from it at the low field region can be observed below TSRT_{\mathrm{SR}} Figure 2(a) and (Figure 2b), indicating a contribution from Δρyx\Delta\rho_{yx}. Figure 2(c) shows the corresponding Hall conductivity Δσxy\Delta\sigma_{xy}, where it only appears below TSRT_{\mathrm{SR}}. With more detailed measurements at intermediate temperatures [36], we construct a contour plot of Δσxy\Delta\sigma_{xy}, which shows a remarkable similarity to those metallic magnets with novel Hall effects [10, 39]. The maximum magnitude of the Hall conductivity at 10 K is about 30 Ω−1cm−1\Omega^{-1}\mathrm{cm}^{-1}, comparable with those in previous “anomalous Hall antiferromagnets” [7]. For magnetic fields applied perpendicular to the kagome plane, however, we do not observe such an AHE [36], suggesting its intimate connection to the magnetic anisotropy as will be discussed below.

As the anomalous electrical transport is closely related to the SR, knowing the change of the magnetic structure across TSRT_{\mathrm{SR}} is crucial to uncovering its origin. We hence use single crystal neutron diffraction to study

the magnetic structure of YbFe6_6Ge6_6. Figure 3(a) shows the diffraction pattern of the (H,0,L)(H, 0, L) plane at 100 K (>TSR> T_{\mathrm{SR}}). There are no additional Bragg peaks except those at integer-index positions, consistent with the well-established A-type AFM structure with a propagation wave vector km=(0,0,0)\mathbf{k}_{\mathrm{m}}=(0, 0, 0) Figure 3(c) [27, 29, 30]. When cooling down to 10 K (<TSR< T_{\mathrm{SR}}), the diffraction pattern is strikingly similar Figure 3(b) - no additional peaks appear, while the peak intensities have clear temperature-dependent behavior due to the SR [36]. This suggests the km\mathbf{k}_{\mathrm{m}} of YbFe6_6Ge6_6 remains to be (0,0,0)(0, 0, 0) below TSRT_{\mathrm{SR}}. Representation analysis based on this propagation wave vector shows only a collinear structure with the spins along the aa-axis Figure 3(d) compatible with the experiment. The SR transition in YbFe6_6Ge6_6 therefore equivalently flips the Néel vector by 90°. More details of the magnetic structure analysis can be found in [36]. The magnetic structure below TSRT_{\mathrm{SR}} along with the lattice space group P6/mmmP6/mmm ensures the system has the T\mathcal{T} symmetry. With small-angle neutron scattering, we also confirmed no field-induced peaks appear under magnetic fields along the a∗a^* direction [36]. These observations rule out that the observed AHE is induced by static spin textures, such as magnetic skyrmions [13], which are restricted by Berry curvature that requires the absence of T\mathcal{T} symmetry [4, 6, 42]. Conversely, the spin-fluctuation driven AHE (or THE) is not necessarily dictated by this symmetry, as it originates from electron scattering by dynamic spins [15, 16, 17, 18].

Neutron diffraction patterns and magnetic structures of the Fe kagome lattice

Figure 3. (a) and (b) Neutron diffraction patterns of the (H,0,L)(H, 0, L) plane at 100 K and 10 K, respectively. The intensity color bar is in log scale to highlight possible weak features. (c) and (d) Magnetic structures of the Fe kagome lattice above and below TSRT_{\mathrm{SR}}, respectively.

Since YbFe6_6Ge6_6 has localized magnetic moments, spin fluctuations below TNT_{\mathrm{N}} are spin waves (magnons), which could impact the motion of conduction electrons [15]. Hence, we use INS to directly probe the magnons and determine their temperature evolution. Figure 4(a) shows the energy dependence of the INS intensities at (0,0,1)(0, 0, 1). At 2.5 K, some INS intensities extend to ∼0.6\sim0.6 meV, which is much larger than our instrumental energy resolution (∼0.14(\sim0.14 meV). Therefore, the spin excitations are gapless in nature. As the temperature increases, their intensity significantly increases, but they remain gapless until 50 K. When the temperature goes beyond TSRT_{\mathrm{SR}}, the intensity of the low-energy part starts to decrease. A broad peak centering around 2 meV shows up at 80 K, indicating the opening of a spin-wave gap. Such gap opening behavior suggests the magnetic anisotropy of YbFe6_6Ge6_6 transfers from an easy-plane type below TSRT_{\mathrm{SR}} to an easy-axis type above TSRT_{\mathrm{SR}}, consistent with the magnetic structures presented in Figure 3(c) and (d). By fitting the data with an error function multiplied by the Bose factor [36, 43], we can extract gap sizes of 0.64(4) meV and 1.34(5) meV at 65 K and 80 K, respectively.

Low-energy spin excitations and temperature dependence of spin fluctuations

Figure 4. (a) Low-energy spin excitations at (0,0,1)(0, 0, 1) at selected temperatures, offset for clarity. Horizontal dashed lines indicate the zero intensity for the data above 2.5 K. Dashed curves are the fits to 65 K and 80 K data [36]. The light blue region shows energy resolution, and the arrow marks 0.6 meV, below which gapless excitations emerge. (b) Temperature dependence of the intensities at (0,0,1)(0, 0, 1) at 0.55 meV and 2.55 meV. (c) Temperature dependence of the maximum magnitudes of Δσxy\Delta\sigma_{xy}. The bold grey curve is a guide to the eyes. Inset illustrates electron scattering by the spin fluctuations.

To determine the evolution of the spin-wave gap, we show the temperature dependence of the intensities at (0,0,1)(0, 0, 1) at 0.55 meV and 2.55 meV [Fig. 4(b)], which are located below and above the spin-wave gap, respectively. Below TSRT_{\mathrm{SR}}, the intensities at both energies increase as the temperature goes up. However, they start to bifurcate at TSRT_{\mathrm{SR}} - while the intensity above the spin-wave gap continues increasing, the intensity below it starts to decrease. The continuous increase of the intensity at 0.55 meV below TSRT_{\mathrm{SR}} further suggests it is an excitation signal rather than the tail of Bragg peak, whose intensity should otherwise decrease when the temperature approaches TSRT_{\mathrm{SR}}. The onset of gapless spin excitations below TSRT_{\mathrm{SR}} aligns with the AHE [see Figure 4(c)], suggesting their correlation.

We point out that the gapless spin excitations below TSRT_{\mathrm{SR}} play a vital role in explaining the AHE through a dynamic SSC scattering mechanism, as first identified in the ferromagnetic heterostructure SrRuO3_3/SrTiO3_3 [31]. The gapless excitations at (0,0,1)(0, 0, 1) within our energy resolution suggests that Fe spins can fluctuate at the cost of a very small energy, facilitating the formation of a dynamic SSC. From a semiclassical perspective, the propagation of spin waves causes adjacent Fe spins in the kagome plane to slightly deviate from the collinear ground state. On the other hand, Yb spins remain disordered above 0.4 K and thus, by themselves, have little impact on the AHE, which emerges at a much higher temperature. However, their interactions with Fe strengthen upon cooling, leading to the TSRT_{\mathrm{SR}} transition. Because the Yb positions and Fe kagome layers are well separated [Fig. 1(a)], the transient non-collinear Fe spin configurations and Yb spins can locally produce an SSC with Si⋅(Sj×Sk)≠0\mathbf{S}_i \cdot(\mathbf{S}_j \times\mathbf{S}_k) \ne0. Despite these local SSCs with opposite signs (++ or −-) cancel out at zero magnetic field due to the global T\mathcal{T} symmetry, a finite magnetic field partially aligns the Yb spins, resulting in a non-zero overall SSC [36]. This non-zero SSC can preferentially scatter electrons and give rise to the observed AHE. However, when the magnetic field becomes exceedingly large, low-energy spin fluctuations are suppressed due to the opening of a Zeeman gap, leading to a vanishing overall SSC and, consequently, a zero AHE. In contrast, the finite spin-wave gap above TSRT_{\mathrm{SR}} suggests relatively high spin stiffness. As a result, Fe spins favor maintaining the ground-state collinear configuration. Both the increased spin stiffness of the Fe kagome layer and the weaker Yb-Fe interaction at higher temperatures are unfavorable for the dynamic SSC, which accounts for the absence of the AHE above TSRT_{\mathrm{SR}}.

Therefore, the AHE in YbFe6_6Ge6_6 can be understood as arising from electron scattering by low-energy spin fluctuations. Given that every Fe ion has a static magnetic moment of approximately 1.5 μB\mu_{\mathrm{B}} below TSRT_{\mathrm{SR}} [36], we estimate a Zeeman gap of roughly 0.6 meV for a 7 T field [43, 44], beyond which the AHE vanishes at low temperatures Figure 2(c) and (d). It suggests the dynamic SSC contributing to the AHE is within 0.6 meV. In addition, this energy scale reasonably matches the gap size at 65 K [Fig. 4(a)], which is slightly above TSRT_{\mathrm{SR}} and the AHE just disappears Figure 4(c). For comparison, we note that the similar kagome antiferromagnet FeSn does not exhibit an AHE [45, 46]. Despite also having a collinear magnetic structure with spins lying in the kagome plane, the spin waves of FeSn display a finite energy gap of ∼2\sim2 meV [47, 48], which suppresses low-energy spin fluctuations.

Recent experiments show that spin fluctuations can give rise to similar AHEs (or THEs) in a range of materials, including single crystals [19, 20, 21, 22, 23, 24, 25, 49, 50] and thin films [31, 51], supporting the idea that spin-fluctuation driven AHE is a general phenomenon. In previous studies, it depends on thermal fluctuations, with samples being heated above or close to the ordering temperature [19, 20, 21, 22, 23, 24, 25, 31, 49, 50, 51]. Those AHEs are therefore essentially driven by paramagnetic spin fluctuations, which are usually dominant around magnetic Bragg peak positions near the transition temperature and are gapless as well [52]. For YbFe6_6Ge6_6, the situation is different. Due to the SR transition induced by the Yb-Fe interaction, the cc-axis aligned spins transfer to the easy-plane arrangement below TSRT_{\mathrm{SR}}, which greatly promotes low-energy spin fluctuations even in the spin-ordered state. With the stronger Yb-Fe interaction at low temperatures, the AHE is enhanced accordingly. Moreover, YbFe6_6Ge6_6 adopts a collinear AFM structure that is much simpler than the magnetic structures of previous single crystals [19, 20, 21, 22, 23, 24, 25, 49, 50]. Our study therefore also suggests that a complex (e.g., chiral) static magnetic structure is not a prerequisite for observing spin-fluctuation driven AHE.

In conclusion, with electrical transport, magnetization, and neutron scattering, we have systematically studied the Fe-based kagome magnet YbFe6_6Ge6_6. An AHE is observed in its AFM-ordered state when the spins are aligned parallel to the kagome plane due to the Yb-Fe interaction. The collinear magnetic structure with ITIT symmetry excludes a static SSC origin of the AHE. By directly measuring the low-energy spin excitations, we find that spin excitations at the Brillouin zone center become gapless in the spin-reorientated state. The simultaneous onset of these gapless excitations and AHE shows their close relationship and points to a dynamic SSC scattering mechanism of the latter. Our results not only reveal a spin-fluctuation driven AHE that is not solely dependent on thermal activation but also demonstrate dynamic spins, even in a collinear antiferromagnet, can significantly impact electrical transport.

Acknowledgments

The neutron scattering and single-crystal synthesis work at Rice was supported by US NSF-DMR-2401084 and by the Robert A. Welch Foundation under grant no. C-1839 (P.D.), respectively. The transport work at University of Tokyo was supported by Grant-in-Aid for Scientific Research (KAKENHI) (JP22H00105), and Grant-in-Aid for Scientific Research on Innovative Areas “Quantum Liquid Crystals” (JP19H05824) from Japan Society for the Promotion of Science. W.Y. acknowledges support from the US NSF-OISE-2201516 under the Accelnet program of Office of International Science and Engineering (OISE). P.D. also acknowledges travel support from the US NSF-OISE-2201516. A portion of this research used resources at the Spallation Neutron Source, a DOE Office of Science User Facility operated by the Oak Ridge National Laboratory. The experiment at the ISIS Neutron and Muon Source was supported by a beam time allocation RB2410134 from the Science and Technology Facilities Council. Ø.S.F. acknowledges funding from the Research Council of Norway through project 325345. This work is in part based on work performed at the DMC instrument at SINQ at the Paul Scherrer Institute. Small-angle neutron scattering was performed at QUOKKA, ANSTO under a proposal number P18792. CLH acknowledges the support by the National Science and Technology Council in Taiwan (NSTC 113-2112-M-006-027). the data shown in Figure 4.

End Matter

Appendix — While dispersive spin waves of YbFe6_6Ge6_6 extend to much higher energies, only the low-energy part (i.e., the spin-wave gap) shows a significant change across TSRT_{\mathrm{SR}}. Figure 5(a) and (b) show the excitation spectra along the [0, 0, LL] direction at 10 K and 100 K, respectively [36]. The signals around L=1L = 1 and 3 are magnons, while phonons appear at larger momentum transfer positions. The overall excitation spectrum changes little except for the intensity, as can be seen from the constant-energy cuts shown in Figure 5(c) and (d). We notice the intensity increase from 10 K to 100 K is significantly larger than the effect simply due to the Bose factor [grey curves in Figure 5(c) and (d)], indicating a change of the spin orientation. Thermal evolution of the low-energy spin excitations around (0, 0, 1) is presented in Figure 5(e)-(i) [36]. Since the magnon has a bandwidth of ∼40\sim40 meV along the [0, 0, LL] direction [36], the spin excitations below 3 meV are rod-like and concentrated at the Brillouin zone center. As the temperature rises to near TSRT_{\mathrm{SR}}, their intensity gradually accumulates, which extends down to the elastic background [Figure 5(e)-(h)]. However, the intensity around 1 meV drops at 80 K (>TSR> T_{\mathrm{SR}}) [Figure 5(i)], indicating the presence of an energy gap, consistent with the data shown in Figure 4.

Excitation spectra and low-energy spin excitations of YbFe6Ge6

Figure 5. (a) and (b) Excitation spectra along [0, 0, LL] direction at 10 K and 100 K, respectively. (c) and (d) Constant energy cuts around (0, 0, 3) at 25 meV and 15 meV, respectively. Grey curves represent the calculated intensities at 100 K by correcting the 10 K data with the Bose factor. (e)-(i) Low-energy spin excitations around (0, 0, 1) at selected temperatures. Magenta arrow indicates the energy gap at 80 K.

Supplemental Material for “Anomalous Electrical Transport in the Kagome Magnet YbFe6_6Ge6_6”

Single crystal growth and characterization

YbFe6_6Ge6_6 single crystals were grown with a Sn-flux method [28]. Raw materials of Yb, Fe, Ge, and Sn powders with a molar ratio of 1 : 1 : 3 : 20 were mixed and loaded into a quartz tube in a glove box. A piece of quartz wool was put in the upper part of the quartz tube before evacuating and sealing. The sealed quartz tube was put into a box furnace and heated to 1100 °C in 24 hours. After keeping at 1100 °C for 10 hours, the quartz tube was gradually cooled at a rate of 5 °C/hour until 500 °C, at which it was flipped and centrifuged to remove excess Sn. YbFe6_6Ge6_6 single crystals in hexagonal or prism can be obtained on the quartz wool, with a typical size of 1∼2 millimeters [see Figure S6(a)]. The crystals were soaked in HCl solution for several days to remove residual Sn. Sharp and clear diffraction spots in the X-ray Laue (Photonic Science) diffraction pattern confirm the high quality of these crystals Figure S6(b). To check the crystal structure, single-crystal X-ray diffraction (XRD) was conducted with the Rigaku Synergy-S diffractometer. Figure S7 shows representative XRD patterns. Crystal structure refinement was performed with the Jana2006 program [53]. The obtained space group is P6/mm ⁣mP6/mm\!m. The comparison between the observed and calculated structure factors is presented in Figure S8. The crystallographic information can be found in Table I and Table II. The chemical elements of our sample were characterized by energy dispersive X-ray spectrum (EDS) in an EMC Helios 660 scanning electron microscope (SEM) (Figure S9). The elemental analysis shown in Table III indicates the chemical elements of our sample are in good agreement with the chemical formula YbFe6_6Ge6_6.

Representative YbFe6Ge6 single crystals and X-ray Laue diffraction pattern

Figure S6. (a) Representative YbFe6_6Ge6_6 single crystals against a millimeter grid. (b) X-ray Laue diffraction pattern taken on the (0, 0, LL) surface.

Single crystal XRD patterns of the (H, K, 0), (H, K, 1), (H, K, 2), and (H, 0, L) planes

Figure S7. Single crystal XRD patterns of the (H,K,0)(H, K, 0), (H,K,1)(H, K, 1), (H,K,2)(H, K, 2), and (H,0,L)(H, 0, L) planes. Arrows represent primitive vectors (a∗\mathbf{a}^{*}, b∗\mathbf{b}^{*}, and c∗\mathbf{c}^{*}) of the reciprocal space.

Calculated structure factor $F_{\mathrm{cal}}$ versus observed structure factor $F_{\mathrm{obs}}$ from single crystal XRD measured at 100 K

Figure S8. Calculated structure factor FcalF_{\mathrm{cal}} versus observed structure factor FobsF_{\mathrm{obs}} from single crystal XRD measured at 100 K.

Energy dispersive X-ray spectrum at a representative spot on a YbFe$_6$Ge$_6$ single crystal

Figure S9. Energy dispersive X-ray spectrum at a representative spot on a YbFe6_6Ge6_6 single crystal. Inset shows the image taken by scanning electron microscopy.

Empirical formulaYbFe6_6Ge6_6
Formula weight943.66
Temperature100.00(10) K
Wavelength0.71073 Å
Crystal systemHexagonal
Space groupP6/mmm
Unit cell dimensionsa=b=5.0795(3)a = b = 5.0795(3) Å, c=8.0806(9)c = 8.0806(9) Å
α=β=90∘\alpha= \beta= 90^\circ, γ=120∘\gamma= 120^\circ
Volume180.56(2) Å3^3
Z1
Density (calculated)8.6070 g·cm−3^{-3}
Absorption coefficient48.511 mm−1^{-1}
F(000)418
Crystal size0.11 × 0.10 × 0.07 mm3^3
Theta range for data collection4.616° to 47.565°
Index ranges−10≤H≤7-10 \le H \le7, −8≤K≤8-8 \le K \le8, −12≤L≤10-12 \le L \le10
Reflections collected1449
Independent reflections310 [R(int) = 0.0279]
Completeness to theta = 25.242°100.0 %
Refinement methodFull-matrix least-squares on F2^2
Data / restraints / parameters310 / 0 / 9
Goodness-of-fit on F2^22.06
Final R indices [I > 3sigma(I)]R1 = 0.0298, wR2 = 0.0749
R indices (all data)R1 = 0.0320, wR2 = 0.0755
Extinction coefficient0.0160(19)

Table I. Crystal data and structure refinement for YbFe6_6Ge6_6.

AtomWyckoff.Occ.xyzUeq_{\mathrm{eq}}
Yb11a10000.0030(2)
Ge12c10.33330.666700.0066(2)
Ge22d10.33330.66670.50.0042(2)
Ge32e1000.3456(2)0.0030(2)
Fe16i10.500.2491(1)0.0032(2)

Table II. Atomic coordinates and equivalent isotropic displacement parameters of YbFe6_6Ge6_6 at 100 K.

ElementWeight percentage (%)Weight percentage error (%)Atomic percentage (%)
Yb18.510.837.75
Fe36.310.7347.13
Ge45.180.7345.12
Total100-100

Table III. Elemental analysis report from the spectrum in Figure S9.

Magnetization measurements

Magnetization measurements up to 9 T were taken with a Quantum Design PPMS system. Pulsed high-field magnetization measurements up to 50 T were performed at Institute for Solid State Physics (ISSP), the University of Tokyo. The absolute magnetizations were normalized according to the magnetization data taken with the Quantum Design PPMS system.

Figure S10 presents the isothermal magnetizations along the cc-axis. At low temperatures below TSRT_{\mathrm{SR}}, the magnetization is almost linear with respect to the field. However, when the temperature goes above TSRT_{\mathrm{SR}}, the magnetization shows a significant slope change, which is due to the field-induced spin reorientation (SR, or spin flop) transition. The transition field gradually increases as the temperature goes up and is larger than 9 T when the temperature is above 100 K, which can be confirmed by the pulsed high-field magnetizations shown in Figure S10. By collecting the transition temperatures at fixed fields and transition fields at fixed temperatures, we construct the phase boundary about cc-axis magnetic field and temperature [Figure S10]. Due to the spontaneous SR transition, the phase boundary ends at the temperature axis. This phase diagram is consistent with the previous report [28]. Note that TSRT_{\mathrm{SR}} does not depend on the magnetic fields applied along the kagome plane (i.e., the phase boundary is parallel to the field axis) [28].

Isothermal and pulsed high-field magnetizations and phase diagram

Figure S10. (a) Isothermal magnetizations along the c-axis up to 9 T at selected temperatures. (b) Pulsed high-field magnetizations along the c-axis up to 50 T at selected temperatures. The oscillation features at high magnetic fields are due to sample vibration at high temperatures (200 K and 250 K). (c) Phase diagram about c-axis magnetic field and temperature. Inset shows the magnetic structures on both sides of the phase boundary.

To check whether the Yb spins order at lower temperatures, additional DC magnetic susceptibility was measured using a Quantum Design MPMS with the He3 option. From Figure S11, we can see the magnetic susceptibility shows a smooth upturning on cooling from 5 K to 0.4 K, which is typical of paramagnetic behavior. Therefore, the Yb spins in this system remain disordered down to 0.4 K, indicating rather weak Yb-Yb interaction. For the magnetic and electrical transport properties above 2 K, which are the focus of the present study, the interaction between Yb and Fe is most relevant.

Temperature dependence of DC magnetic susceptibility

Figure S11. Temperature dependence of DC magnetic susceptibility from 0.4 K to 5 K under a field of 0.1 T applied parallel to the c-axis.

Electrical transport measurements

Electrical transport measurements up to 9 T were performed in a Quantum Design PPMS system. Electrical transport measurements up to 12 T were performed in a cryogen-free superconducting magnet (TeslatronPT, Oxford) with a homemade stick. YbFe6_6Ge6_6 single crystals were cut and polished into an approximately rectangular shape before making electrical contacts. The typical sample size in our transport measurement is about 1×0.5×0.15 mm31 \times0.5 \times0.15\ \mathrm{mm}^3. Contact misalignment was corrected by field symmetrizing and anti-symmetrizing the longitudinal and transverse resistance data, respectively.

Electrical transport under in-plane magnetic fields

Magnetoresistance (MR) and Hall measurements at 14 temperatures were shown in Figure S12 and Figure S13, which include the data shown in Figure 2(a) and (b) of the main text. The magnetic fields were applied along the a∗a^* direction. We use a two-band model to simultaneously fit the MR and Hall data above 6 T [38, 40, 41], according to which the longitudinal and transverse resistivities can be written as

Field dependence of longitudinal resistivity at selected temperatures

Figure S12. Field dependence of longitudinal resistivity at selected temperatures with the field applied along the a* direction. The electric current is along the b-axis. Dashed curves are the fits with the two-band model.

Hall resistivity at selected temperatures with the field applied along the $a^{*}$ direction

Figure S13. Hall resistivity at selected temperatures with the field applied along the a∗a^{*} direction. Dashed curves are the fits with the two-band model.

ρxxO(B)=1e(nhμh+neμe)+(nhμe+neμh)μhμeB2(nhμh+neμe)2+(nh−ne)2μh2μe2B2(1)\rho_{xx}^{O}(B) = \frac{1}{e}\frac{(n_h\mu_h+n_e\mu_e)+(n_h\mu_e+n_e\mu_h)\mu_h\mu_eB^2}{(n_h\mu_h+n_e\mu_e)^2+(n_h-n_e)^2\mu_h^2\mu_e^2B^2} \tag*{(1)}

and

ρyxO(B)=1e(nhμh2−neμe2)+(nh−ne)μh2μe2B2(nhμh+neμe)2+(nh−ne)2μh2μe2B2B,(2)\rho_{yx}^{O}(B) = \frac{1}{e} \frac{(n_h\mu_h^2-n_e\mu_e^2)+(n_h-n_e)\mu_h^2\mu_e^2B^2}{(n_h\mu_h+n_e\mu_e)^2+(n_h-n_e)^2\mu_h^2\mu_e^2B^2}B, \tag*{(2)}

where ee represents the elementary charge, nhn_h and nen_e are the carrier densities of the hole-like and electron-like bands, respectively, and μh\mu_h and μe\mu_e are the corresponding mobilities. The fitted results are shown as the dashed curves in Figure S12 and Figure S13. The temperature dependences of the mobility and carrier density are presented in Figure S14. Below TSRT_{\mathrm{SR}}, the hole-like band has a larger mobility than the electron-like band, but its carrier density is much smaller than the latter. Such behavior is not uncommon in metals with magnetic rare earth ions [54, 55]. As the temperature increases, the difference between the two kinds of bands narrows, indicating the weakened impact of the rare earth ion (Yb3+^{3+}) [28] and the material becomes closer to a one-band-like system at high temperature. An anomaly appears around TSRT_{\mathrm{SR}}, which is consistent with the SR transition and the derivative of resistivity [Fig. 1(b) of the main text]. Here we need to point out that the actual electronic structure of YbFe6_6Ge6_6 might be much more complex than a two-band system. For these electrical transport measurements, no hysteresis can be discerned between field ramp-up and ramp-down. For example, the Hall resistivities measured from +12 T to -12 T and -12 T to +12 T basically overlap with each other [see Figure S15]. The anomalous Hall resistivity is obtained by subtracting the fitted curve of the two-band model (ordinary Hall resistivity ρyxo\rho^{\mathrm{o}}_{yx})

Temperature dependence of the mobility and carrier density

Figure S14. Temperature dependence of the mobility (a) and carrier density (b) obtained from the two-band model fit.

Hall resistivity at 10 K

Figure S15. Hall resistivity at 10 K measured from +12 T to -12 T (blue) and from -12 T to +12 T (orange). The dashed curve is the fit with the two-band model.

Δρyx=ρyx−ρyxo.(3)\Delta\rho_{yx}=\rho_{yx}-\rho^{\mathrm{o}}_{yx}. \tag*{(3)}

The anomalous Hall conductivity presented in Figure 2(c) and (d) of the main text is approximately calculated as

Δσxy=Δρyxρxx2+ρyx2.(4)\Delta\sigma_{xy}=\frac{\Delta\rho_{yx}}{\rho_{xx}^{2}+\rho_{yx}^{2}}. \tag*{(4)}

To further confirm the observed anomalous Hall effect (AHE), additional electrical transport measurements were conducted with the Quantum Design PPMS system. Figure S16 presents detailed Hall resistivities from 50 K to 70 K. In this temperature region, the curved multi-band feature is evident even for fields below 9 T, which enables us to fit the data with a two-band model. Below TSRT_{\mathrm{SR}}, we can clearly see that the Hall resistivity at low field deviates from the curve of the two-band model. This deviation, however, gradually smears out as the temperature goes up. Figure S16 shows an enlarged view of the data and the fit at 56 K. The resultant fitting parameters are shown in Figure S16 and (d), which are reasonably consistent with the data measured up to 12 T (Figure S14).

Hall resistivity and two-band model fit

Figure S16. (a) Hall resistivity from 50 K to 70 K with 1 K per step. Magnetic field up to ±9\pm9 T is applied along the a∗a^{*} direction. The electric current is along the bb-axis. Dashed curves are the fits with the two-band model. Data above 50 K are offset by 0.01 μΩ⋅\mu\Omega\cdotcm for clarity. (b) Same data at 56 K in (a). (c) and (d) Temperature dependence of the mobility and carrier density of the two-band model fit.

The observed AHE below TSRT_{\mathrm{SR}} can be understood through a dynamic scalar spin chirality (SSC) scattering mechanism, which is schematically illustrated by Figure S17. Due to the existence of the Yb spins and their increased interaction with the Fe kagome lattice below TSRT_{\mathrm{SR}}, two adjacent Fe spins can form a spin triad with the out-of-plane Yb spin (yellow triangles in Figure S17). When considering the fluctuations of the Fe spins from a semiclassical perspective, they will deviate from the static collinear state. So this kind of Yb-Fe spin triad can have non-zero SSC. Without

Anomalous Hall conductivity and spin configurations

Figure S17. Anomalous Hall conductivity Δσxy\Delta\sigma_{xy} at 10 K. Insets schematically show the behaviors of the spin configurations of Yb (cyan) and Fe (red), respectively, at various magnetic fields, as indicated by the blue arrows. Yellow triangles (“1” and “2”) highlight two spin triads of Yb-Fe. Light red arrows represent the static magnetic structure below TSRT_{\mathrm{SR}}. Light red circles indicate the “easy plane” for the Fe spins. Spin canting angles are exaggerated for better visualization.

an external magnetic field, these local SSCs will cancel out due to the combined space inversion and time-reversal (ITIT) symmetry. For example, in Figure S17, spin triad 1 has negative SSC χ1<0\chi_1 < 0, but spin triad 2, connected by the global ITIT symmetry, has a positive SSC χ2>0\chi_2 > 0 with the same magnitude. These local SSCs therefore do not contribute an overall SSC, i.e., ∑iχi≈0\sum_i \chi_i \approx0, which results in the absence of AHE at zero field.

Applying a magnetic field slightly aligns the Yb spins to the field direction, which breaks the balance between positive and negative SSCs, despite low-energy spin fluctuations being slightly suppressed by the field. The static Fe spin orientation is almost not affected by the field, as the energy scale of Fe-Fe interaction is much larger than the magnetic field. This produces a net overall SSC (∑iχi≠0\sum_i \chi_i \ne0) so that gives rise to an AHE. However, when the magnetic field becomes very large, low-energy spin fluctuations are significantly suppressed by opening a Zeeman gap. The spin fluctuation induced SSC, along with the accompanied AHE, then vanishes again. This process qualitatively explains the field dependence of the observed AHE. Here, the change of spin anisotropy in YbFe6_6Ge6_6 is critical, where the Yb-Fe interaction at low temperatures triggers the change of spin anisotropy and gives rise to the gapless spin excitations. Spin anisotropy change is also found to be important for the spin-fluctuation driven AHE in the ferromagnetic heterostructure SrRuO3_3/SrTiO3_3 [31]. However, in that case, it is due to the thermal fluctuation near the ferromagnetic transition temperature, which is different from our case.

Electrical transport under out-of-plane magnetic fields

Figure S18 shows the Hall resistivity ρzx\rho_{zx} at selected temperatures from 10 K to 100 K under cc-axis magnetic fields. Although the Hall resistivity is largely linear with respect to the field, it shows slope change for temperatures above TSRT_{\mathrm{SR}}, as can be more clearly seen in Figure S19. This is similar to the magnetization data of this field direction [Figure S10 in Section II]. Note that for high temperatures, the slope change of ρzx\rho_{zx} is expected to occur at magnetic fields larger than 9 T, which is beyond our measurements. Such behavior indicates a non-negligible contribution to the Hall effect from the net magnetization along the cc-axis.

Hall resistivity at selected temperatures

Figure S18. Hall resistivity at selected temperatures with the field applied along the cc-axis. Dashed curves are the fits as described in the text.

Hall resistivity at 50 K, 70 K, and 100 K

Figure S19. Hall resistivity at 50 K, 70 K, and 100 K with the field applied along the cc-axis. Dashed curves are the fits as described in the text. Inset shows the Hall measurement configuration and the definition of xx, yy, and zz axes. (b) Temperature dependence of the Hall coefficient R0R_0 obtained from the fitting.

We find the measured ρzx\rho_{zx} can be well fitted with the following equation

ρzx=ρzxO+ρzxA,(5)\rho_{zx} = \rho_{zx}^{\mathrm{O}} + \rho_{zx}^{\mathrm{A}}, \tag*{(5)}

where ρzxO\rho_{zx}^{\mathrm{O}} is ordinary Hall resistivity and ρzxA\rho_{zx}^{\mathrm{A}} is conventional anomalous Hall resistivity due to net magnetization. They can be written as

ρzxO=R0B(6)\rho_{zx}^{\mathrm{O}} = R_{0}B \tag*{(6)}

and

ρzxA=SAM.(7)\rho_{zx}^{\mathrm{A}} = S_{\mathrm{A}}M. \tag*{(7)}

R0R_{0} is the ordinary Hall coefficient and SAS_{\mathrm{A}} is another proportional coefficient. Since both the Hall resistivity and magnetization are almost proportional to the magnetic field at low and high temperatures (i.e., 10 K, 30 K, 50 K, 100 K, and 110 K), we cannot determine R0R_{0} and SAS_{\mathrm{A}} separately. To add constraints, we assume SAS_{\mathrm{A}} is temperature independent [4] and simultaneously fit the data at 9 temperatures. The fitted results are shown as the dashed curves in Figure S18 and Figure S19. The ordinary Hall coefficient R0R_{0} is shown in Figure S19 and SAS_{\mathrm{A}} is 1.12(2) μΩ⋅cm⋅μB−1⋅Fe\mu\Omega\cdot\mathrm{cm}\cdot\mu_{\mathrm{B}}^{-1}\cdot\mathrm{Fe}.

Therefore, no additional spin-fluctuation driven AHE contributes to the ρzx\rho_{zx}, where the magnetic field is applied along the cc-axis. This observation is similar to other kagome magnets with easy-plane magnetic structures - AMn6_6Sn6_6 (A = Y, Sc, and Er) [19, 21, 22] and HoAgGe [25], where the spin-fluctuation driven AHEs can only be observed when the magnetic fields are applied along the kagome plane. It suggests that these AHEs are primarily contributed by in-plane spin fluctuations [19, 21, 22, 25], which are suppressed by an out-of-plane field as the spins tilt away from the magnetic easy plane.

Neutron diffraction and analysis of the magnetic structure

Neutron diffraction measurements

Neutron diffraction measurements were conducted with the CORELLI diffractometer at Spallation Neutron Source, Oak Ridge National Laboratory [56] and the DMC diffractometer at Swiss Spallation Neutron Source (SINQ), Paul Scherrer Institut. One piece of YbFe6_6Ge6_6 single crystal with a mass of about 15 mg was used in these two experiments, respectively.

Fig. S20(a) shows the temperature dependence of the diffraction intensity at (0,0,1)(0, 0, 1). We can see the intensity abruptly drops when the temperature goes above TSR≈63T_{\mathrm{SR}} \approx63 K, which is due to the disappearance of the spin component along the cc-axis. At the Bragg peak (1, 0, 1), the intensity shows a canonical order-parameter behavior with respect to the temperature [Figure S20], consistent with the ordering temperature TN≈500T_{\mathrm{N}} \approx500 K. These temperature-dependent

Temperature dependence of diffraction intensities for Bragg peaks (0, 0, 1) and (1, 0, 1)

Figure S20. Temperature dependence of the diffraction intensities for Bragg peaks (0, 0, 1) (a) and (1, 0, 1) (b), where arrows indicate TSRT_{\mathrm{SR}} and TNT_{\mathrm{N}}, respectively.

data were taken at the CORELLI diffractometer. The absence of additional Bragg peaks below TSRT_{\mathrm{SR}} can be further confirmed by the diffraction pattern taken at (H,H,L)(H,H,L) plane Figure S21, which corroborates the observation that neither charge order nor incommensurate magnetic order occurs below TSRT_{\mathrm{SR}}. Diffraction maps presented in Figure 3 of the main text and Figure S21 were taken with the DMC diffractometer.

Neutron diffraction patterns for the (H, H, L) plane at 100 K and 10 K

Figure S21. Neutron diffraction patterns for the (H,H,L)(H,H,L) plane taken on a piece of YbFe6_6Ge6_6 single crystal at 100 K (a) and 10 K (b), respectively. The intensity color bar is in log scale to highlight possible weak features.

Analysis of the magnetic structure

With the magnetic propagation wave vector km=(0,0,0)\mathbf{k}_{\mathrm{m}}=(0,0,0) in hand, we can do representation analysis to get possible magnetic structures [57]. For this purpose, we use the BasIReps program implemented in the FullProf suite [58]. The magnetic representation Γmag\Gamma_{\mathrm{mag}} of the Fe ion located at (0.5,0,zFe)(0.5,0,z_{\mathrm{Fe}}) (with zFe=0.2491z_{\mathrm{Fe}}=0.2491) for space group P6/mmmP6/mmm can

be decomposed as

Γmag=1Γ12+1Γ13+1Γ14+1Γ25+2Γ26+1Γ17+1Γ19+1Γ110+1Γ211+2Γ212.(8)\Gamma_{\mathrm{mag}} = 1\Gamma_{1}^{2} + 1\Gamma_{1}^{3} + 1\Gamma_{1}^{4} + 1\Gamma_{2}^{5} + 2\Gamma_{2}^{6} + 1\Gamma_{1}^{7} + 1\Gamma_{1}^{9} + 1\Gamma_{1}^{10} + 1\Gamma_{2}^{11} + 2\Gamma_{2}^{12}. \tag*{(8)}

The irreducible representations (IRs) and their basis vectors (BVs) are listed in Table IV. Assuming Fe ions have the same magnetic moment size, we can construct all possible magnetic structures from these BVs, which are explicitly shown in Figure S16. Among them, ferromagnetic structures Ψ1\Psi_{1} [Figure S16] and Ψ8−Ψ9\Psi_{8}-\Psi_{9} [Figure S16] are irrelevant to the magnetic structure of YbFe6_6Ge6_6, which is an antiferromagnet. Ψ10\Psi_{10} [Figure S16] corresponds to the A-type antiferromagnetic structure between TNT_{\mathrm{N}} and TSRT_{\mathrm{SR}}. For the remaining 7 configurations, their magnetic structure factors at Bragg peak positions can be directly calculated and compared with the (integrated) intensities obtained from neutron diffraction.

IRBVFe1Fe2Fe3Fe4Fe5Fe6
Γ2\Gamma_{2}Ψ1\Psi_{1}(0,0,1)(0,0,1)(0,0,1)(0,0,1)(0,0,1)(0,0,1)
Γ3\Gamma_{3}Ψ2\Psi_{2}(1,0,0)(0,1,0)(-1,-1,0)(1,0,0)(0,1,0)(-1,-1,0)
Γ4\Gamma_{4}Ψ3\Psi_{3}(0.5,1,0)(-1,-0.5,0)(0.5,-0.5,0)(0.5,1,0)(-1,-0.5,0)(0.5,-0.5,0)
Γ5\Gamma_{5}Ψ4\Psi_{4}(0,0,0)(0,0,-1)(0,0,1)(0,0,0)(0,0,-1)(0,0,1)
Ψ5\Psi_{5}(0,0,1)(0,0,-0.5)(0,0,-0.5)(0,0,1)(0,0,-0.5)(0,0,-0.5)
Ψ6\Psi_{6}(0.5,1,0)(0.5,0.25,0)(-0.25,0.25,0)(0.5,1,0)(0.5,0.25,0)(-0.25,0.25,0)
Γ6\Gamma_{6}Ψ7\Psi_{7}(0,0,0)(0,-1,0)(-1,-1,0)(0,0,0)(0,-1,0)(-1,-1,0)
Ψ8\Psi_{8}(0,0,0)(-1,-0.5,0)(-0.5,0.5,0)(0,0,0)(-1,-0.5,0)(-0.5,0.5,0)
Ψ9\Psi_{9}(1,0,0)(0,-0.5,0)(0.5,0.5,0)(1,0,0)(0,-0.5,0)(0.5,0.5,0)
Γ7\Gamma_{7}Ψ10\Psi_{10}(0,0,1)(0,0,1)(0,0,1)(0,0,-1)(0,0,-1)(0,0,-1)
Γ9\Gamma_{9}Ψ11\Psi_{11}(0.5,1,0)(-1,-0.5,0)(0.5,-0.5,0)(-0.5,-1,0)(1,0.5,0)(-0.5,0.5,0)
Γ10\Gamma_{10}Ψ12\Psi_{12}(1,0,0)(0,1,0)(-1,-1,0)(-1,0,0)(0,-1,0)(1,1,0)
Γ11\Gamma_{11}Ψ13\Psi_{13}(0,0,0.5)(0,0,-1)(0,0,0.5)(0,0,-0.5)(0,0,1)(0,0,-0.5)
Ψ14\Psi_{14}(0,0,-1)(0,0,0)(0,0,1)(0,0,1)(0,0,0)(0,0,-1)
Γ12\Gamma_{12}Ψ15\Psi_{15}(1,0,0)(0,-0.5,0)(0.5,0.5,0)(-1,0,0)(0,0.5,0)(-0.5,-0.5,0)
Ψ16\Psi_{16}(0,0,0)(1,0.5,0)(0.5,-0.5,0)(0,0,0)(-1,-0.5,0)(-0.5,0.5,0)
Ψ17\Psi_{17}(0,0,0)(0,1,0)(1,1,0)(0,0,0)(0,-1,0)(-1,-1,0)
Ψ18\Psi_{18}(0.5,1,0)(0.5,0.25,0)(-0.25,0.25,0)(-0.5,-1,0)(-0.5,-0.25,0)(0.25,-0.25,0)

Table IV. Irreducible representations (IRs) and basis vectors (BVs) for the space group P6/mmmP6/mmm with magnetic propagation vector km=(0,0,0)\mathbf{k}_{m}=(0,0,0).

In neutron diffraction, the integrated intensity of a magnetic Bragg peak is proportional to the modulus square of the magnetic structure factor [59]

IM(Q)=AdσMdΩ∣Q=ANM(2π)3VM∣FM(Q)∣2,(9)I_{\mathrm{M}}(\mathbf{Q}) = A \left.\frac{d\sigma_{\mathrm{M}}}{d\Omega}\right|_{\mathbf{Q}} = A N_{\mathrm{M}}\frac{(2\pi)^3}{V_{\mathrm{M}}}\lvert F_{\mathrm{M}}(\mathbf{Q})\rvert^2, \tag*{(9)}

where NMN_{\mathrm{M}} is the number of magnetic unit cells in the sample, VMV_{\mathrm{M}} is the volume of the magnetic unit cell. The magnetic structure factor can be written as

FM(Q)=∑jγr02gjfj(Q)S⊥jeiQ⋅rje−Wj.(10)F_{\mathrm{M}}(\mathbf{Q}) = \sum_j \frac{\gamma r_0}{2}g_j f_j(\mathbf{Q})\mathbf{S}_{\perp j}e^{i\mathbf{Q}\cdot\mathbf{r}_j}e^{-W_j}. \tag*{(10)}

S⊥j\mathbf{S}_{\perp j} is the spin size at site jj that is detectable by neutrons

S⊥j=Sj−Q^(Q^⋅Sj),(11)\mathbf{S}_{\perp j} = \mathbf{S}_j - \hat{\mathbf{Q}}(\hat{\mathbf{Q}}\cdot\mathbf{S}_j), \tag*{(11)}

where Q^\hat{\mathbf{Q}} is the unit vector of Q\mathbf{Q} and Sj\mathbf{S}_j is the spin vector at site jj. The magnetic moment at site jj in Bohr magneton is gjSjg_j\mathbf{S}_j. The term γr02\frac{\gamma r_0}{2} in (10) containing the classical electron radius (r0r_0) and gyromagnetic ratio (γ\gamma) acts as an effective scattering length of per Bohr magneton, which is 2.695 fm [59].

For magnetic structures with the spins lying in the kagome plane, their magnetic structure factor at (0,0,1)(0, 0, 1) can be explicitly written as

FM(Q)=γr02gf(Q)[(S1+S2+S3)ei2πzFe+(S4+S5+S6)e−i2πzFe],(12)F_{\mathrm{M}}(\mathbf{Q}) = \frac{\gamma r_{0}}{2} g f(\mathbf{Q}) \left[(\mathbf{S}_{1}+\mathbf{S}_{2}+\mathbf{S}_{3})e^{i2\pi z_{\mathrm{Fe}}}+(\mathbf{S}_{4}+\mathbf{S}_{5}+\mathbf{S}_{6})e^{-i2\pi z_{\mathrm{Fe}}}\right], \tag*{(12)}

where we have assumed the same gg-factor and magnetic form factor for all Fe ions and taken e−Wj≈1e^{-W_{j}}\approx1. S1\mathbf{S}_{1}, S2\mathbf{S}_{2}, and S3\mathbf{S}_{3} are the three spins in the first layer of the unit cell, and S4\mathbf{S}_{4}, S5\mathbf{S}_{5}, and S6\mathbf{S}_{6} are the three spins in the second layer (see Figure S22). According to equation (12), we can immediately see that the magnetic structure factor at (0,0,1)(0, 0, 1) vanishes for Ψ2\Psi_{2}, Ψ3\Psi_{3}, Ψ8+Ψ9\Psi_{8}+\Psi_{9}, Ψ11\Psi_{11}, Ψ12\Psi_{12}, and Ψ17+Ψ18\Psi_{17}+\Psi_{18} [Figure S22-(Figure S22) and (g)-(i)], where S1+S2+S3=0\mathbf{S}_{1}+\mathbf{S}_{2}+\mathbf{S}_{3}=0 and S4+S5+S6=0\mathbf{S}_{4}+\mathbf{S}_{5}+\mathbf{S}_{6}=0 establish. On the contrary, our neutron diffraction experiment shows that significant magnetic scattering emerges at (0,0,1)(0, 0, 1) below TSRT_{\mathrm{SR}} (see Figure S20, Figure S21, and Figure 3 of the main text). Such observation excludes these 6 configurations and makes Ψ17−Ψ18\Psi_{17}-\Psi_{18} [Figure S22] the only possible magnetic structure below TSRT_{\mathrm{SR}}. Based on the magnetic structure Ψ17−Ψ18\Psi_{17}-\Psi_{18}, it is straightforward to calculate its magnetic scattering intensities and compare them with the experiment. Figure S23, (Figure S23), (Figure S23), and (Figure S23) show the integrated intensities of a series of Bragg peaks at 80 K and 4 K. The data were taken at the CORELLI diffractometer, which can cover a large reciprocal space based on the Laue method. The difference of the integrated intensities between the two temperatures is shown in Figure S23, (Figure S23), (Figure S23), and (Figure S23), which can be satisfactorily fitted with the magnetic structure Ψ17−Ψ18\Psi_{17}-\Psi_{18} [Figure S22]. The resultant magnetic moment per Fe ion is

Possible magnetic structures of the Fe kagome lattice

Figure S22. Possible magnetic structures of the Fe kagome lattice based on the representation analysis.

Integrated intensities and corresponding differences of Bragg peaks along four reciprocal-space directions

Figure S23. (a), (c), (e), and (g) Integrated intensities of Bragg peaks along [0, 0, LL], [1, 0, LL], [2, 0, LL], and [1, 1, LL], respectively, at 80 K and 4 K. (b), (d), (f), and (h) The corresponding differences of the integrated intensities between 4 K and 80 K. The vertical orange bars indicate the calculated intensities from the determined magnetic structure. Inset of (h) is a zoom-in view of the data in the magenta box.

MFe=gSμB=1.51(3)μB.(13)M_{\mathrm{Fe}} = gS\mu_{\mathrm{B}} = 1.51(3)\mu_{\mathrm{B}}. \tag*{(13)}

This moment size is consistent with previous reports [26, 27, 29].

Possible non-collinear magnetic structure

Non-collinear magnetic structures have been observed in many kagome magnets. For instance, the B35 structure FeGe exhibits a non-collinear “double-cone” structure [44]. Notably, this compound can be regarded as the parent material of YbFe6_{6}Ge6_{6}. So it would be useful to estimate the upper bound of a possible non-collinear magnetic structure for YbFe6_{6}Ge6_{6}.

Figure S24 presents the diffraction profiles around (0,0,1)(0, 0, 1) along the [0,0,L][0, 0, L] and [H,0,1][H, 0, 1] directions, from which we can confirm the absence of additional peaks below TSRT_{\mathrm{SR}}. Any satellite peak, if it exists, should be 3∼4 orders of magnitude weaker than the major magnetic Bragg peak (i.e., in the level of the background). For comparison, the incommensurate magnetic peaks in FeGe (which are indicators of non-collinear magnetic structure) are about one order of magnitude weaker than the major magnetic peaks [44].

Figure S24. Diffraction profiles along the [0, 0, LL] and [HH, 0, 1] directions at 10 K and 100 K, which are obtained from the data shown in Figure 2(a) and (b) of the main text. Solid curves are the fits with Gaussian profiles. Insets of (a) and (c) show the same data with the intensity in log scale.

To quantitatively estimate the upper bound of a possible non-collinear magnetic structure, we first assume the non-collinearity is a helical type [60, 61] - the spin rotates a small angle with respect to its neighbors. Figure S25 schematically shows a cc-axis helical structure supposed on the AA-type antiferromagnetic structure, where the spins are perpendicular to the cc-axis. This structure will result in a satellite magnetic Bragg peak at Q+(0,0,δ)\mathbf{Q}+(0, 0, \delta), with

Schematic of a c-axis helical structure supposed on the planar A-type antiferromagnetic structure

Figure S25. Schematic of a cc-axis helical structure supposed on the planar AA-type antiferromagnetic structure. Each arrow represents a spin perpendicular to the cc-axis. Two neighboring spins span a turn angle α+180∘\alpha+ 180^\circ.

δ=2/(2π/α)\delta= 2/(2\pi/\alpha). α+180∘\alpha+ 180^\circ is the turn angle spanned by two neighboring spins along the helical axis (i.e., the cc-axis), where α\alpha directly quantifies the non-collinearity of two spins.

Although we do not observe separate satellite peaks in YbFe6_6Ge6_6, they could be very close to integer-index positions so that cannot be resolved from the major peak. At 10 K, the full-width-at-half-maximum (FWHM) of the (0, 0, 1) peak is 0.0203(1) (in reciprocal lattice unit) along the [0, 0, LL] direction [Figure S24]. That means for a possible satellite peak, the length of its propagation wave vector δ\delta should be smaller than 0.0203. Therefore, the angle α\alpha is smaller than 3.65°. Similarly, based on the FWHM along the [HH, 0, 1] direction [Figure S24], we can estimate the upper bound of α\alpha to be 0.76° for spins in this direction. In the case of FeGe, an in-plane helical component is superposed on the axial A-type antiferromagnetic structure, which gives the “double-cone” structure [62]. The turn angle α+180∘\alpha+ 180^\circ for the in-plane helical component is 194.4° and α=14.4∘\alpha= 14.4^\circ [62].

Possible field-induced magnetic structure and small-angle neutron scattering

It has been widely recognized that field-induced static spin structures may give rise to AHE (or topological Hall effect). These structures usually have incommensurate propagation wave vectors of relatively small size, with the magnetic skyrmion as the most well-known example. To test whether this is the case for the observed AHE in YbFe6_6Ge6_6, we first estimate the real-space periodicity of the possible field-induced magnetic structure. Under this scenario, the anomalous Hall resistivity is proportional to the emergent magnetic field [63, 64]

Δρyx=PR0b,(14)\Delta\rho_{yx} = P R_0 b, \tag*{(14)}

where PP is the spin polarization, R0R_0 is the ordinary Hall coefficient, and bb is the emergent magnetic field. Spin polarization can be obtained from the magnetization data [63]

P=MMsat,(15)P = \frac{M}{M_{\mathrm{sat}}}, \tag*{(15)}

where MsatM_{\mathrm{sat}} is the saturated magnetic moment. R0R_0 can be estimated from the fitted result of the ordinary Hall contribution (see Section II). On the other hand, the emergent magnetic field bb is related to the real-space periodicity of the magnetic structure with the following formula [64]

∣b∣≈ϕ0λ2,(16)|b| \approx\frac{\phi_0}{\lambda^2}, \tag*{(16)}

where ϕ0=he\phi_0 = \frac{h}{e} is the flux quantum and λ\lambda is the periodicity of the magnetic structure in real space. By combining (14), (15), and (16), we can get

λ≈ϕ0MR0MsatΔρyx.(17)\lambda\approx\sqrt{\frac{\phi_0 M R_0}{M_{\mathrm{sat}}\Delta\rho_{yx}}}. \tag*{(17)}

For a magnetic field of 3 T, around which the AHE is most significant, we estimate λ≈200 A˚\lambda\approx200\,\text{\AA}. This real-space periodicity corresponds to a propagation wave vector in the order of q∼0.03 A˚−1q \sim0.03\,\text{\AA}^{-1} in reciprocal space. The emergent magnetic field b≈12b \approx12 T.

We use small-angle neutron scattering (SANS) to explore possible field-induced magnetic structures with such real-space periodicity. Our SANS experiment was performed with the QUOKKA instrument at the Australian Nuclear Science and Technology Organisation [65]. The sample is a 15 mg YbFe6_6Ge6_6 single crystal. We attached Cd plates with a hole of ∼2.5\sim2.5 mm diameter on the sample holder to reduce scattering from the background. The sample holder was loaded into a horizontal field superconducting magnet. The direction of the magnetic field was parallel to the a∗\mathbf{a}^{*} direction. Incident neutron beam with a wavelength of 5 A˚\text{\AA} was parallel to the cc-axis. We used low-qq and high-qq setups to cover momentum transfers from 0.008 A˚−1\text{\AA}^{-1} to 0.04 A˚−1\text{\AA}^{-1} and from 0.045 A˚−1\text{\AA}^{-1} to 0.146 A˚−1\text{\AA}^{-1}, respectively.

Figure S26(a) and (b) present the SANS patterns at 10 K, 0 T and 10 K, 3 T, respectively, where we do not see Bragg peak in the range from 0.008 A˚−1\text{\AA}^{-1} to 0.03 A˚−1\text{\AA}^{-1} and the two patterns do not show a significant difference. These observations can be confirmed from the azimuthally averaged SANS intensities as a function of momentum transfer from 0.008 A˚−1\text{\AA}^{-1} to 0.04 A˚−1\text{\AA}^{-1} [Figure S26(c)]. Moreover, with the high-qq setup, there is still no evident difference for the data at 10 K, 0 T and 10 K, 3 T [Figure S26(d)]. Therefore, we can rule out field-induced magnetic Bragg peaks in the momentum transfer from 0.008 A˚−1\text{\AA}^{-1} to 0.14 A˚−1\text{\AA}^{-1}.

SANS patterns and azimuthally averaged intensities

Figure S26. (a) and (b) SANS patterns at 10 K, 0 T and 10 K, 3 T measured with the low-qq setup. (c) and (d) Azimuthally averaged SANS intensities as a function of momentum transfer in the low-qq and high-qq setups, respectively.

As discussed above, if the observed AHE is due to field-induced static spin texture, the corresponding propagation wave vector is expected to be in the order of q∼0.03 A˚−1q \sim0.03\,\text{\AA}^{-1}. So, the absence of field-induced peaks from 0.008 A˚−1\text{\AA}^{-1} to 0.14 A˚−1\text{\AA}^{-1} makes it very unlikely that the AHE is due to field-induced static spin textures.

Inelastic neutron scattering

Inelastic neutron scattering (INS) experiments with time-of-flight neutron spectrometers were performed on a coaligned single crystal array with the ARCS spectrometer at Spallation Neutron Source, Oak Ridge National Laboratory [66] and the MERLIN spectrometer at ISIS Spallation Neutron Source, the Rutherford Appleton Laboratory [67]. The obtained time-of-flight neutron data was reduced and analyzed with Mantid [68] and HORACE [69]. An additional INS experiment was performed on the same sample with the cold neutron spectrometer HODACA at Japan Research Reactor-3 (JRR3) [70]. The coaligned single crystal array is shown in Figure S27(a), which consists of about 1000 pieces (∼0.9\sim0.9 gram) of small single crystals glued on two aluminum plates. The samples on the plates were oriented such that the scattering plane was (H,0,L)(H, 0, L). For the time-of-flight neutron scattering data shown in the presented figures, their momentum- and/or energy-integrated ranges are listed in Table V.

Coaligned single crystals and rocking scans

Figure S27. (a) Coaligned single crystals used in our INS experiments. (b) and (c) Rocking scans performed at Bragg peaks (0,0,2)(0, 0, 2) and (2,0,0)(2, 0, 0), respectively. Solid lines are the fits with Gaussian profiles.

DataMomentum-integrated range (r.l.u.)Energy-integrated range (meV)Spectrometer
Figure 5(a) and (b)[-0.1, 0.1] along [H,0,0][H, 0, 0] [-0.1, 0.1] along [−0.5K,−K,0][-0.5K, -K, 0]-ARCS
Figure 5(c) and (d)[-0.1, 0.1] along [H,0,0][H, 0, 0] [-0.1, 0.1] along [−0.5K,−K,0][-0.5K, -K, 0][-1, 1]ARCS
Figure 5(e)-(i)[-0.1, 0.1] along [H,0,0][H, 0, 0] [-0.1, 0.1] along [−0.5K,−K,0][-0.5K, -K, 0]-MERLIN
Figure S29[-0.1, 0.1] along [H,0,0][H, 0, 0] [-0.1, 0.1] along [−0.5K,−K,0][-0.5K, -K, 0][-1, 1]ARCS
Figure S30(a)-(d)[-0.1, 0.1] along [H,0,0][H, 0, 0] [-0.1, 0.1] along [−0.5K,−K,0][-0.5K, -K, 0]-ARCS
Figure S30(e) and (f)[-0.2, 0.2] along [0,0,L][0, 0, L][-5, 5]ARCS
Figure S31[-0.15, 0.15] along [0,0,L][0, 0, L][-1, 1]MERLIN

Table V. Momentum- and/or energy-integrated ranges for the INS data presented in figures.

Excitation spectra and constant energy cuts

Figure S30. (a) and (b) Excitation spectra along [0,0,L]\left[0, 0, L\right] at 10 K and 100 K, respectively. (c) and (d) Excitation spectra along [H,0,3]\left[H, 0, 3\right] at 10 K and 100 K, respectively. (e) and (f) Constant energy cuts around 40 meV of the (H,K,3)\left(H, K, 3\right) plane at 10 K and 100 K, respectively. White hexagons are the Brillouin zone boundaries.

The data shown in Figure 4(a) and (b) of the main text were measured at the HODACA spectrometer, which was run in the triple-axis mode. Rocking scans performed at Bragg peaks (0,0,2)(0, 0, 2) and (2,0,0)(2, 0, 0) indicate a sample mosaic spread of 0.40(1)∘0.40(1)^\circ and 0.34(2)∘0.34(2)^\circ, respectively [Figure S27 and (c)], which are estimated by their FWHMs. For INS measurements, constant energy scans at fixed momentum positions were performed with a fixed final neutron energy of Ef=3.636E_f = 3.636 meV. The energy resolution is about 0.140.14 meV at zero energy transfer. The typical counting time for each energy position is about 5 minutes. Additional INS data taken above 100 K are shown in Figure S28, which supplement the data presented in Figure 4(a) of the main text. To extract the energy gap size, we fit these data with an error function multiplied by the Bose factor [43]

Low-energy spin excitations and temperature dependence of the fitted gap size

Figure S28. (a) Low-energy spin excitations around (0,0,1)(0, 0, 1) at selected temperatures above 100 K. Data are evenly offset for clarity. Dashed curves are the fits as described in the text. (b) Temperature dependence of the fitted gap size. The fitting errorbar is smaller than the symbol size.

I(E,T)=[I0+A⋅erf⁡(E−Egapσ)]⋅11−e−E/kBT,(18)I(E,T) = \left[I_0 + A \cdot\operatorname{erf}\left(\frac{E-E_{\mathrm{gap}}}{\sigma}\right)\right]\cdot\frac{1}{1-e^{-E/k_{\mathrm{B}}T}}, \tag*{(18)}

where erf⁡(x)\operatorname{erf}(x) represents the error function, I0I_0, AA, σ\sigma, and EgapE_{\mathrm{gap}} (the gap size) are fitting parameters. The fitting results are shown with dashed curves in Figure 4(a) of the main text and Figure S28. The obtained gap sizes at various temperatures are presented in Figure S28. From 65 K to 300 K, we can see that the spin-wave gap size gradually increases, which is consistent with the increase of the spin-flop field above TSRT_{\mathrm{SR}} [see the phase diagram in Figure S10] [28].

The data shown in Figure 5(a)-(Figure 5d) of the main text were measured at the ARCS spectrometer with an incident neutron energy (EiE_i) of 40 meV. The energy resolution is about 2.4 meV at zero energy transfer. The sample was rotated along the [−0.5K,K,0][-0.5K, K, 0] direction for about 150∘150^\circ in 1∘1^\circ per step. The counting time for each sample rotation angle is about 6 minutes. To reveal the different dependence behaviors of the phonon and magnon, constant energy cuts around (0,0,8)(0, 0, 8) along the [0,0,L][0, 0, L] direction are presented in Figure S20. These signals mainly come from phonons due to the large momentum transfer. We can see that the intensity change between 10 K and 100 K follows the Bose factor, which is in contrast to the magnon signals shown in Figure 5(c) and (d) of the main text. Figure S29 presents more INS data of 10 K and 100 K measured with Ei=100E_i = 100 meV, from which we can see the higher energy part of the magnon emanating from (0,0,3)(0, 0, 3). The spin-wave bandwidth is about 40 meV for the dispersion perpendicular to the kagome plane, and is larger than 60 meV along the kagome plane. In these measurements, the energy resolution is about 8 meV at zero energy transfer.

Figure S29. (a) and (b) Constant energy cuts around (0,0,8)(0, 0, 8) along the [0,0,L][0, 0, L] direction at 10 meV and 20 meV, respectively. Grey curves represent the calculated intensities at 100 K by correcting the 10 K data with the Bose factor.

The data shown in Figure 5(e)-(Figure 5i) of the main text were measured at the MERLIN spectrometer with Ei=15E_i = 15 meV. The energy resolution is about 0.7 meV at zero energy transfer. Since the low-energy magnetic excitations concentrate very close to the Brillouin zone center, we rotated the sample along the [−0.5K,K,0][-0.5K, K, 0] direction for about 60∘60^\circ in 1∘1^\circ per step. The measured reciprocal space covers a region along the [0,0,L][0, 0, L] direction. The counting time for each sample rotation angle is about 14 minutes. Figure S31 presents the distribution of the low-energy spin excitations in the hexagonal Brillouin zone, which confirms the rod-like feature shown in Figure 5(e)-(Figure 5i) of the main text.

Constant energy cuts of low-energy spin excitations

Figure S31. (a)-(e) Constant energy cuts of the low-energy spin excitations at selected temperatures. Data are obtained by integrating the energy from 1 meV to 3 meV. Only the data of the first hexagonal Brillouin zone centering at (0,0,1)\left(0, 0, 1\right) are shown.

References

  1. [1]E. H. Hall, American Journal of Mathematics 2, 287 (1879).
  2. [2]E. H. Hall, Philosophical Magazine 12, 157 (1881).
  3. [3]G. Bergmann, Physics Today 32, 25 (1979).
  4. [4]N. Nagaosa, J. Sinova, S. Onoda, A. H. MacDonald, and N. P. Ong, Rev. Mod. Phys. 82, 1539 (2010).
  5. [5]S. Nakatsuji, N. Kiyohara, and T. Higo, Nature 527, 212 (2015).
  6. [6]H. Chen, Q. Niu, and A. H. MacDonald, Phys. Rev. Lett. 112, 017205 (2014).
  7. [7]L. Šmejkal, A. H. MacDonald, J. Sinova, S. Nakatsuji, and T. Jungwirth, Nature Reviews Materials 7, 482 (2022).
  8. [8]E. V. Gomonay and V. M. Loktev, Low Temperature Physics 40, 17 (2014).
  9. [9]N. Kanazawa, Y. Onose, T. Arima, D. Okuyama, K. Ohoyama, S. Wakimoto, K. Kakurai, S. Ishiwata, and Y. Tokura, Phys. Rev. Lett. 106, 156603 (2011).
  10. [10]T. Kurumaji, T. Nakajima, M. Hirschberger, A. Kikkawa, Y. Yamasaki, H. Sagayama, H. Nakao, Y. Taguchi, T.-h. Arima, and Y. Tokura, Science 365, 914 (2019).
  11. [11]M. Hirschberger, T. Nakajima, S. Gao, L. Peng, A. Kikkawa, T. Kurumaji, M. Kriener, Y. Yamasaki, H. Sagayama, H. Nakao, K. Ohishi, K. Kakurai, Y. Taguchi, X. Yu, T.-h. Arima, and Y. Tokura, Nature Communications 10, 5831 (2019).
  12. [12]G. Kimball, C. Kim, W. Wu, M. Cuoco, and J. W. Robinson, Communications Materials 3, 19 (2022).
  13. [13]N. Nagaosa and Y. Tokura, Nature Nanotechnology 8, 899 (2013).
  14. [14]The distinction between “anomalous Hall effect” and “topological Hall effect” in the literature is not unambiguous. Sometimes, anomalous Hall effect is broadly used to refer topological Hall effect, as also noted by [12]. In this paper, since we do not discuss the topological property, we use anomalous Hall effect to refer the Hall effect other than the ordinary one.
  15. [15]S. A. Yang, H. Pan, Y. Yao, and Q. Niu, Phys. Rev. B 83, 125122 (2011).
  16. [16]W.-T. Hou, J.-X. Yu, M. Daly, and J. Zang, Phys. Rev. B 96, 140403 (2017).
  17. [17]H. Ishizuka and N. Nagaosa, Science Advances 4, eaap9962 (2018).
  18. [18]H. Ishizuka and N. Nagaosa, Phys. Rev. B 103, 235148 (2021).
  19. [19]N. J. Ghimire, R. L. Dally, L. Poudel, D. Jones, D. Michel, N. T. Magar, M. Bleuel, M. A. McGuire, J. Jiang, J. Mitchell, J. W. Lynn, and I. I. Mazin, Science Advances 6, eabe2680 (2020).
  20. [20]Q. Wang, K. J. Neubauer, C. Duan, Q. Yin, S. Fujitsu, H. Hosono, F. Ye, R. Zhang, S. Chi, K. Krycka, H. Lei, and P. Dai, Phys. Rev. B 103, 014416 (2021).
  21. [21]H. Zhang, C. Liu, Y. Zhang, Z. Hou, X. Fu, X. Zhang, X. Gao, and J. Liu, Applied Physics Letters 121, 202401 (2022).
  22. [22]K. Fröhling, A. Streeter, S. Mardanya, X. Wang, P. Baral, O. Zaharko, I. I. Mazin, S. Chowdhury, W. D. Ratcliff, and F. Tafti, Phys. Rev. Mater. 8, 094411 (2024).
  23. [23]K. K. Kolincio, M. Hirschberger, J. Masell, S. Gao, A. Kikkawa, Y. Taguchi, T. Hira, A. Nagaosa, and Y. Tokura, Proceedings of the National Academy of Sciences 118, e2023588118 (2021).
  24. [24]K. K. Kolincio, M. Hirschberger, J. Masell, T.-h. Arima, N. Nagaosa, and Y. Tokura, Phys. Rev. Lett. 130, 136701 (2023).
  25. [25]S. Roychowdhury, K. Samanta, S. Singh, W. Schnelle, Y. Zhang, J. Noky, M. G. Vergniory, C. Shekhar, and C. Felser, Proceedings of the National Academy of Sciences 121, e2401970121 (2024).
  26. [26]G. Venturini, R. Welter, and B. Malaman, Journal of Alloys and Compounds 185, 99 (1992).
  27. [27]T. Mazet and B. Malaman, Journal of Physics: Condensed Matter 12, 1085 (2000).
  28. [28]M. A. Avila, T. Takabatake, Y. Takahashi, S. L. Bud’ko, and P. Canfield, Journal of Physics: Condensed Matter 17, 6969 (2005).
  29. [29]J. M. Cadogan and D. H. Ryan, Journal of Physics: Condensed Matter 22, 016009 (2009).
  30. [30]D. H. Ryan, J. M. Cadogan, and R. Gagnon, Journal of Physics: Conference Series 217, 012124 (2010).
  31. [31]W. Wang, M. W. Daniels, Z. Liao, Y. Zhao, J. Wang, G. Koster, G. Rijnjders, C.-Z. Chang, D. Xiao, and W. Wu, Nature Materials 18, 1054 (2019).
  32. [32]T. Mazet, O. Isnard, and B. Malaman, Solid State Communications 114, 91 (2000).
  33. [33]T. Mazet and B. Malaman, Journal of Alloys and Compounds 325, 67 (2001).
  34. [34]T. Mazet, V. Ban, R. Sibille, S. Capelli, and B. Malaman, Solid State Communications 159, 79 (2013).
  35. [35]G. Venturini, Zeitschrift für Kristallographie-Crystalline Materials 221, 511 (2006).
  36. [36]See Supplemental Material [url] for additional data and analyses, which includes Refs. [53–70].
  37. [37]N. Kumar, Y. Soh, Y. Wang, and Y. Xiong, Phys. Rev. B 100, 242240 (2019).
  38. [38]L. Wang, J. Zhu, H. Chen, H. Wang, J. Liu, Y.-X. Huang, B. Jiang, J. Zhao, H. Shi, G. Tian, H. Wang, Y. Yao, D. Yu, Z. Wang, C. Xiao, S. A. Yang, and X. Wu, Phys. Rev. Lett. 132, 106601 (2024).
  39. [39]T. Suzuki, R. Chisnell, A. Devarakonda, Y.-T. Liu, W. Feng, D. Xiao, J. W. Lynn, and J. G. Checkelsky, Nature Physics 12, 1119 (2016).
  40. [40]N. W. Ashcroft and N. D. Mermin, Solid State Physics (Holt-Saunders, New York, 1976).
  41. [41]Z. Zhu, B. Fauqué, K. Behnia, and Y. Fuseya, Journal of Physics: Condensed Matter 30, 313001 (2018).
  42. [42]X.-Y. Hou, H.-C. Yang, Z.-X. Liu, P.-J. Guo, and Z.-Y. Lu, Phys. Rev. B 107, L161109 (2023).
  43. [43]L. Chen, X. Teng, H. Tan, B. L. Winn, G. E. Granroth, F. Ye, D. H. Yu, R. A. Mole, B. Gao, B. Yan, M. Yi, and P. Dai, Nature Communications 15, 1918 (2024).
  44. [44]X. Teng et al., Nature 609, 490 (2022).
  45. [45]B. C. Sales, J. Yan, W. R. Meier, A. D. Christianson, S. Okamoto, and M. A. McGuire, Phys. Rev. Mater. 3, 114203 (2019).
  46. [46]M. Kang et al., Nature Materials 19, 163 (2020).
  47. [47]Y. Xie, L. Chen, T. Chen, Q. Wang, Q. Yin, J. R. Stewart, M. B. Stone, L. L. Daemen, E. Feng, H. Cao, H. Lei, Z. Yin, A. H. MacDonald, and P. Dai, Communications Physics 4, 240 (2021).
  48. [48]S.-H. Do, K. Kaneko, K. Kajimoto, K. Kamazawa, M. B. Stone, J. Y. Y. Lin, S. Itoh, T. Masuda, G. D. Samolyuk, E. Dagotto, W. R. Meier, B. C. Sales, H. Miao, and A. D. Christianson, Phys. Rev. B 105, L180403 (2022).
  49. [49]N. Abe, Y. Hano, H. Ishizuka, Y. Kozuka, T. Tadano, Y. Tsujimoto, K. Yamaura, S. Ishiwata, and J. Fujioka, npj Quantum Materials 9, 41 (2024).
  50. [50]H. Jeon, H. Seo, J. Seo, Y. H. Kim, E. S. Choi, Y. Jo, H. N. Lee, J. M. Ok, and J. S. Kim, Communications Physics 7, 162 (2024).
  51. [51]Y. Fujishiro, N. Kanazawa, R. Kurihara, H. Ishizuka, T. Hori, F. S. Yasin, X. Yu, A. Tsukazaki, M. Ichikawa, M. Kawasaki, N. Nagaosa, M. Tokunaga, and Y. Tokura, Nature Communications 12, 317 (2021).
  52. [52]M. F. Collins and W. Marshall, Proceedings of the Physical Society 92, 390 (1967).
  53. [53]V. Petříček, M. Dušek, and L. Palatinus, Zeitschrift für Kristallographie - Crystalline Materials 229, 345 (2014).
  54. [54]L. Ye, T. Suzuki, and J. G. Checkelsky, Phys. Rev. B 95, 174405 (2017).
  55. [55]D. Ram, J. Singh, M. K. Hooda, O. Pavlosiuk, V. Kanchana, Z. Hossain, and D. Kaczorowski, Phys. Rev. B 107, 085137 (2023).
  56. [56]F. Ye, Y. Liu, R. Whitfield, R. Osborn, and S. Rosenkranz, Journal of Applied Crystallography 51, 315 (2018).
  57. [57]A. Wills, J. Phys. IV France 11, Pr9 (2001).
  58. [58]J. Rodríguez-Carvajal, Physica B: Condensed Matter 192, 55 (1993).
  59. [59]G. Shirane, S. M. Shapiro, and J. M. Tranquada, Neutron scattering with a triple-axis spectrometer: basic techniques (Cambridge University Press, 2002).
  60. [60]D. C. Johnston, Phys. Rev. Lett. 109, 077201 (2012).
  61. [61]D. C. Johnston, Phys. Rev. B 96, 104405 (2017).
  62. [62]J. Bernhard, B. Lebech, and O. Beckman, Journal of Physics F: Metal Physics 14, 2379 (1984).
  63. [63]A. Neubauer, C. Pfleiderer, B. Binz, A. Rosch, R. Ritz, P. G. Niklowitz, and P. Böni, Phys. Rev. Lett. 102, 186602 (2009).
  64. [64]Y. Tokura and N. Kanazawa, Chemical Reviews 121, 2857 (2021).
  65. [65]K. Wood et al., Applied Crystallography 51, 294 (2018).
  66. [66]D. L. Abernathy, M. B. Stone, M. J. Loguillo, M. S. Lucas, O. Delaire, X. Tang, J. Y. Y. Lin, and B. Fultz, Review of Scientific Instruments 83, 015114 (2012).
  67. [67]R. Bewley, R. Eccleston, K. McEwen, S. Hayden, M. Dove, S. Bennington, J. Treadgold, and R. Coleman, Physica B: Condensed Matter 385-386, 1029 (2006).
  68. [68]O. Arnold et al., Nuclear Instruments and Methods in Physics Research Section A: Accelerators, Spectrometers, Detectors and Associated Equipment 764, 156 (2014).
  69. [69]R. Ewings, A. Buts, M. Le, J. van Duijn, I. Bustinduy, and T. Perring, Nuclear Instruments and Methods in Physics Research Section A: Accelerators, Spectrometers, Detectors and Associated Equipment 834, 132 (2016).
  70. [70]H. Kikuchi, S. Asai, T. J. Sato, T. Nakajima, L. Harriger, I. Zaliznyak, and T. Masuda, Journal of the Physical Society of Japan 93, 091004 (2024).

Paper details

vlnc:W_rcphpkt8
Version
v1 · latest
Published
Fresh — added to the Hub within the last 30 days
Added
License
CC BY 4.0
Usage

views · 7

downloads · 0

A view counts once per browser per day, a download each time the PDF is requested.

  • Physics and Astronomy

Not recorded for this paper

View statement
Looking for related papers…
Contents