WorksPhysics and Astronomy
Electrothermal behavior of superconducting nanowires buried in a commercial CMOS process
Abstract
Superconducting films native to a commercial CMOS process enable co-integration of superconducting devices (high-kinetic-inductance elements and nanowire detectors) with cryogenic CMOS on one monolithic die. Such films are buried in the front-end-of-line, beneath the back-end-of-line metal stack, an environment that might quench a self-heated hot spot. Current-voltage characteristics are reported for titanium nitride (TiN) nanowires in the polycrystalline-silicon resistor layer of a 22 nm FD-SOI process, and measured retrapping currents are compared with thermal models for longitudinal conduction to the contacts and interfacial phonon cooling into the stack. The wires are strongly hysteretic, with switching-to-retrapping current ratios I_sw/I_r of 7.4-9.8, sustaining a normal hot spot. For two wires of length ell = 50 micrometers and widths W = 0.50 and 1.00 micrometers, over bath temperatures T_b = 0.15-1.19 K, I_r follows the interfacial form (T_hs^n - T_b^n)^(1/2) with n = 4 (T_hs, the effective hot-spot temperature), and is strongly inconsistent with the (T_hs - T_b)^(1/2) constant-kappa longitudinal-conduction limit; free-exponent fits give n = approximately 4.8-5.0. An effective cooling coefficient Sigma_K = 7.9(3) W/(m^2 K^4) describes the data: 31(21) times below the acoustic- (diffuse-) mismatch value for a single clean interface, and approximately 12 times below the lowest previously reported comparable nanowire coefficient. The model-based film thermal conductivity is kappa = approximately 20 mW/(m K). Across lengths ell = 1-50 micrometers, I_r matches neither ell^(-1) of pure longitudinal conduction nor ell^0 of pure interfacial cooling; a two-channel model reproduces I_r(ell) with crossover length ell* = approximately 3.5 micrometers predicted, to an O(1) prefactor, from Sigma_K and kappa.
Commercial complementary metal oxide semiconductor (CMOS) processes routinely use transition-metal nitrides and silicides as diffusion barriers, liner metals and passive components.[1, 2, 3] Several become superconducting at cryogenic temperatures[4, 5, 6, 7]—a property incidental to processes designed for room-temperature operation, in which the films are chosen for work function, adhesion and sheet resistance. Recently Swift et al. used one such film as a circuit element.[8] They exploited the high kinetic inductance (≈ 1 nH per square) of the titanium nitride (TiN) sub-film inside a polycrystalline-silicon resistor (poly-resistor) of a GlobalFoundries 22 nm fully depleted silicon-on-insulator (FD-SOI) process. The resulting “superinductor” is four orders of magnitude more compact in area than the spiral inductors conventionally available on such a process. It is used to read out a silicon metal–oxide–semiconductor (MOS) quantum dot in an integrated radio-frequency single-electron transistor, establishing the film as a usable circuit material for superconductor-enhanced CMOS circuits.
The significance extends beyond passive inductors. The disordered superconductors of exactly this class (e.g., TiN, NbN, NbTiN, WSi) are the workhorse materials of superconducting nanowire single-photon detectors[9, 10, 11] and of nanowire logic and memory.[12, 13, 14] They are chosen for the same properties that make them good superconductors: high normal-state resistivity, short coherence length and low electron diffusivity. A CMOS process that natively contains such a film is therefore a candidate platform for monolithically integrating nanowire detectors and superconducting logic and memory circuits with their cryogenic CMOS readout electronics.
The environment of the film matters for that prospect. The front end of line (FEOL) contains the transistor-level structures at the wafer surface—active silicon, isolation, gate stack and silicide—while the back end of line (BEOL) is the multilevel metal-and-dielectric interconnect built on top of it. The TiN layer studied here is a few-nanometer-thick film within the body of a poly-resistor.[15] It lies on shallow-trench-isolation oxide and is capped by doped polysilicon, silicided at the contact ends. Above it the pre-metal dielectric separates the FEOL from the first metal level of the BEOL stack.[8] The TiN layer is buried in the FEOL beneath the BEOL stack, encapsulated in amorphous dielectric with oxide below and metal interconnects and density fill above (Figure 1).

Figure 1. Cross-section along the wire, not to scale. The TiN film lies on the shallow-trench-isolation (STI) oxide, is capped by doped polysilicon with silicide over the two contact ends, and is buried under the pre-metal dielectric (PMD), the BEOL metal levels (M1, M2), and inter-metal dielectric (IMD); isolated M1/M2 blocks are floating density fill, and dots mark where the stack continues. A hot spot at loses heat along the film to the contacts (set by ) and vertically into the surrounding layers (set by ). is the length between the silicide pads; runs into the page.
The buried environment makes the electrothermal behavior of the TiN film uncertain. In superconducting nanowire detectors, photon absorption can nucleate a transient resistive region whose subsequent evolution (e.g., collapse, growth, or latching) is governed by electrothermal feedback,[11, 16, 17] related feedback is also exploited in nanowire logic and memory.[12, 13, 14] The retrapping current —required to sustain an existing normal (resistive) domain—lies below the switching current at which a cold superconducting wire becomes resistive. Whereas is governed by superconducting-instability mechanisms such as depairing, phase slips, or vortex entry, is determined by heat removal. Whether a film buried close to the BEOL metal stack can sustain a hot spot is therefore not obvious from its geometry alone and requires experimental characterization together with electrothermal modeling.
Heat can leave the hot spot by two routes, which are considered separately. A retrapping current is defined for longitudinal conduction along the film to the contacts, while a distinct retrapping current is defined for interfacial cooling from the film into the surrounding stack. Unadorned denotes the measured retrapping current. Because the resistive hot spot is not isothermal, its interior can be warmer than even though the normal–superconducting boundaries occur near . Accordingly, is treated as an effective hot-spot temperature and fitted to the measured ,[18] rather than being fixed at .
First, consider longitudinal conduction.[19] In the symmetric one-dimensional limit, a normal domain of length , occupying a fraction of the wire, has resistance , while the remaining superconducting material forms two arms of length that conduct to contacts held at the bath temperature . Each arm conducts away from the hot spot, so the two together remove ; equating this to the Joule power gives . Since is maximized at , where it equals , the smallest current that can sustain a stationary hot spot is
where is the wire cross-sectional area, is the normal-state resistance of the full wire, is the sheet resistance, and is an effective along-film thermal conductivity over the temperature range of the superconducting arms (Figure 1). If varies with temperature, the factor in Eq. (1) is replaced by .[19] Equation (1) therefore represents the constant- or temperature-averaged- limit of longitudinal cooling, rather than a universal temperature dependence for heat conduction along the wire.
Second, vertical phonon-mediated cooling removes heat from the film into the surrounding stack,[18, 20] with an effective areal flux and . For a normal segment of length , both the Joule power and the vertical cooling power scale with ; the segment length therefore cancels, giving:
Heat taking this route leaves the film through two parallel vertical paths: downward through the amorphous dielectric toward the silicon handle, and upward through the doped polysilicon cap. The downward path is expected to dominate, as the upward one meets the poor sub-kelvin conductivity of the polysilicon and pre-metal dielectric and ends largely in floating metal fill rather than a dedicated heat sink. As used here, is therefore an effective stack-level coefficient per unit TiN area: it folds several series bottlenecks—multiple interfaces, transport through amorphous dielectric, and the absence of a dedicated upper heat sink—into a single number, and is not the microscopic thermal-boundary conductance of any individual interface.
The TiN films are found in poly-resistor structures in a GlobalFoundries 22 nm FD-SOI process.[8] The wires studied here have and an assumed film thickness .[15, 21] Four-point – measurements were performed on two devices of width and , both of length , on one die, at bath temperatures ranging from to . The measured normal-state sheet resistance is .
and are defined as the largest positive currents within the zero-voltage band on the up-sweep and down-sweep branches respectively; the band is set to 2% of the full-scale voltage. is reproducible sweep to sweep. is not: it varies because some individual sweeps switch prematurely at lower currents. The values quoted below are therefore the maxima measured over the low-temperature plateau, .
Figure 2 shows that the wires enter a self-sustaining resistive state, hysteretic between the switching and retrapping currents. The narrow device gives and , a ratio of 9.8. The wide device gives and , a ratio of 7.4.
Figure 2. Hysteretic current–voltage characteristics of TiN nanowires, , at . (a) : the up-sweep switches at and the down-sweep retraps at . (b) : , . Vertical dotted lines mark the extracted currents. Each above is that of the single trace shown; because individual sweeps scatter downward through premature switching, the text instead quotes the maximum over the plateau. Thresholds are taken on the positive branch; agrees between polarities to within 4%.
Averaged over the measured bath-temperature range, –, the measured ratio is , consistent with the linear scaling in shared by and . The temperature dependence, by contrast, differs between the two models: both give , with for the constant- longitudinal-conduction limit and for the conventional interfacial phonon-radiation model. Fitting with and both free parameters decisively rejects the constant- longitudinal-conduction limit, while (interfacial phonon radiation) follows the measurements over the full bath-temperature range, – (Figure 3). Allowing the exponent itself to float returns and for the two devices. An explicit fit follows the temperature dependence better than (RMS residual 0.9–1.5% versus 1.4–1.8%). Nevertheless, the two parameterizations give nearly equal cooling fluxes that differ by less than 3% at , indicating that the inferred magnitude of heat removal is insensitive to this choice. The form is retained as the conventional phonon-radiation parameterization for direct comparison with Ref. 18 and the acoustic- and diffuse-mismatch benchmarks. Because the TiN film is ultrathin, reduced-dimensional phonon modes could in principle modify the temperature dependence of the conventional three-dimensional phonon-radiation model. The fitted exponent – shows no evidence for a reduced-exponent regime over the measured temperature range, although the exponent alone does not uniquely identify the microscopic thermal bottleneck.
Figure 3. normalized to its 0.15 K value against , for both devices, with fitted in the prefactor and the hot-spot temperature and normalized at the same point, for (constant- longitudinal-conduction limit), 2, and 4 (conventional interfacial phonon-radiation model). Among the fixed exponents shown, best follows the data over the full range.
Setting equal to the measured and rearranging Eq. (2) gives
Here, is fitted independently for the two devices in the model, yielding and for and , respectively. Their mean, , is then held fixed when is evaluated point-by-point at each measured for both devices. The 62 points below yield , with no resolved systematic dependence on temperature or width (Figure 4). The parenthetical uncertainty is the sample standard deviation of the point-by-point values, while the corresponding standard error is approximately .
Figure 4. Effective cooling (Kapitza) coefficient extracted point by point from Eq. (2) for both devices. The 62 extractions below give one temperature-independent value, (solid line), 31(21) below the tabulated acoustic- (diffuse-) mismatch value for a single clean TiN/SiO interface [18].
Equivalently, comparison of the fitted form
with Eq. (2) gives
The fitted prefactors independently give and for the two devices, consistent with the point-by-point mean. Thus, the point-by-point extraction also provides a consistency check that the effective cooling coefficient is independent of and .
For TiN on SiO, Ref. 18 tabulates ideal thermal-boundary coefficients of for the acoustic-mismatch model[22] and for the diffuse-mismatch model[23]. These single-interface values exceed the effective cooling coefficient extracted for the buried CMOS stack by factors of 31(21) for the acoustic- (diffuse-) mismatch model. A fairer clean-limit benchmark for a buried film is the dominant downward stack of Figure 1: combining the thermal resistances of the layers and interfaces in series gives ideal effective coefficients of (acoustic-mismatch) and (diffuse-mismatch), corresponding to factors of 8.0(6.5) above the measured for the acoustic- (diffuse-) mismatch model. Dane et al. fitted for 15 single-layer NbN nanowires on six substrates and obtained values consistent with the acoustic-mismatch prediction [18]. The buried CMOS TiN film measured here lies a factor of 12 below the lowest effective cooling coefficient among those 15 directly comparable wires.
What has been established so far applies to long wires. For , is set by vertical phonon-mediated cooling into the surrounding stack (Figure 4). Conduction to the contacts scales with the cross-section while vertical cooling scales with the footprint , so their relative importance scales primarily with , making wire length the experimental control parameter for the crossover. The data that follow instead vary at fixed , spanning – at and , measured at [24].
Where the crossover falls is set by the film thermal conductivity. It is estimated using the expressions of Ref. 18, combining a Bardeen–Rickayzen–Tewordt electronic contribution[25] with the normal-state Wiedemann–Franz conductivity and a Casimir-limit phonon contribution. Given a measured sheet resistance , the inferred normal-state resistivity is , which is in turn used for the Wiedemann–Franz electronic thermal conductivity . For , the resulting model-based estimate is , of the order measured in other superconducting thin films at sub-Kelvin temperatures[26].
An independent retrapping-current analysis by Swift, performed assuming , yielded [24]. Rescaling that estimate to while keeping the measured gives , of the same order as the present model-based value. Since the electronic contribution dominates, the product entering Eqs. (3) and (5) is nearly independent of the assumed film thickness.
Treating longitudinal conduction and vertical cooling together requires the introduction of the linearized thermal healing length [27, 28], which is the distance heat spreads along the film before it escapes vertically into the surrounding stack:
with the measured , exponent , and computed . A hot spot much longer than loses its heat vertically into the surrounding stack and never reaches the contacts. One shorter than a few loses an appreciable fraction longitudinally, out through the contacts at either end, and needs more current to sustain itself. therefore increases at shorter lengths and plateaus at longer ones. Combining the two limiting loss terms into a single compact interpolation gives the two-channel form :
with estimated from the and fixed above. Equation (4) is phenomenological: it lumps the hot spot into a single temperature rather than solving for the profile along the wire, and the prefactor in Eq. (5) is a heuristic constant carried over from the single-channel hot-spot profile, so is an order-of-magnitude prediction. For it returns the length-independent of Eq. (2). For the contacts dominate and it recovers the scaling of Eq. (1), with an amplitude that depends on the hot-spot profile assumed.
Equation (4) is applied to these structures in Figure 5. The data fall steeply over the first decade of length, roll over at a few micrometres, and are flat by ; the two widths run parallel, separated by their width ratio. Equation (4) is fitted to each width with two free parameters, the plateau current and the crossover length . The fits return and and and . The plateau currents agree with the and obtained from the measurements, and the fitted agrees with the predicted to within the prefactor of Eq. (5). The unusually long crossover follows directly from the weak vertical cooling: at fixed , , and , Eq. (5) gives . Three cooling coefficients therefore set three crossover lengths. The measured gives . The ideal buried stack, , gives . A single clean interface, , gives , quoted throughout for the acoustic- (diffuse-) mismatch model. This benchmark is derived here from Eq. (5), not a crossover length measured by Ref. 18. An otherwise similar film with conventional strong vertical thermal coupling would therefore reach its rollover at a wire length about six times shorter: stronger vertical cooling removes heat within a shorter healing length , which shortens and moves the knee in to shorter wires. The 2-D substrate model gives a characteristic lateral spreading length of approximately , well above the to wire-length range studied here. The substrate therefore acts as an approximately uniform thermal bath over the measured devices, and the few-micrometer crossover is instead set by the competition between longitudinal conduction along the TiN film and vertical cooling into the surrounding stack.
Figure 5. Length dependence of across the TiN test structures of Ref. 24, measured at . Markers are measured data. Solid curves are Eq. (4) with amplitude and fitted per width; dotted lines are the corresponding interfacial floors.
The extracted depends on the modeling conventions used to reduce the data, chiefly the hot-spot-temperature assignment. The extraction relation constrains only the product , so the inferred coefficient scales inversely with the assumed thermal driving term. The headline value follows the fitted- convention of Ref. 18, for which the fit of Figure 3 gives , slightly above . Fixing and refitting the two devices instead gives .
Wire width constitutes a separate systematic uncertainty because ; for example, a reduction in the assumed width would increase the inferred coefficient by approximately . The reported extraction nevertheless uses the drawn device widths throughout and does not assume a narrower effective current-carrying channel. Thus, the same retrapping data yield or approximately , depending on the hot-spot-temperature convention, reflecting modeling uncertainty rather than distinct physical cooling coefficients. The latter value remains approximately below the acoustic- (diffuse-) mismatch value for a single clean TiN/SiO interface, compared with for the headline fitted- value. The inferred coefficients also remain below the range reported for NbN by Ref. 18. Electron-phonon nonequilibrium was also assessed using the two-temperature model of Ref. 18, in which the electron-phonon heat flux is , with parameterized following Refs. 18 and 29. Using an order-of-magnitude TiN coupling estimate together with the measured , , and the fitted gives and a differential electron-phonon conductance approximately ten times the film-to-bath conductance. These numerical values are estimates for the present film. Published TiN electron-phonon relaxation times vary substantially,[30] so this calculation is used only as an order-of-magnitude consistency check.
In summary, TiN nanowires buried in the FEOL beneath the BEOL stack of a commercial CMOS process sustain self-heated hot spots with hysteresis ratios of –. Transient hot-spot formation underpins nanowire detection; controlled hysteresis, nanowire logic and memory. Retrapping in the long wires is governed by vertical phonon-mediated cooling into the surrounding stack rather than by longitudinal conduction to the contacts. A single effective cooling coefficient, , describes the data under the conventional parameterization. Over a fiftyfold range of length, follows neither the longitudinalconduction limit nor the vertical-cooling limit, but crosses between them at a few micrometres (fitted 4.4 to 4.6 µm), near the two-channel crossover µm predicted from the measured and the computed . The unusually small effective therefore explains both the low long-wire retrapping current and the extended length scale over which contact cooling remains important.
Acknowledgments
This work was supported by the U.S. Department of Energy, Office of Science, Advanced Scientific Computing Research (ASCR), High Energy Physics (HEP) and Basic Energy Sciences (BES), under Contract No. DE-AC02-06CH11357 at Argonne. Work performed at the Advanced Photon Source, a U.S. Department of Energy Office of Science User Facilities (SUF). Work at University of Chicago is supported by the Divisions of Chemistry (CHE) and Materials Research (DMR), National Science Foundation, under grant numbers NSF/CHE-1834750 and NSF/CHE-2335833. M.F.G.Z. acknowledges a UKRI Future Leaders Fellowship [MR/V023284/1]. A.G.-S. acknowledges an Industrial Fellowship from the Royal Commission for the Exhibition of 1851. This work was primarily supported by the CMOS+X project funded by DOE’s Genesis Mission.
Author Declarations
Conflict of Interest
The authors have no conflicts to disclose.
Author Contributions
Mohamed Gharib: Methodology (equal); Software (equal); Formal analysis (lead); Writing – original draft (equal); Writing – review & editing (equal); Visualization (lead). Leonid Popryho: Software (equal); Validation (lead); Writing – review & editing (equal). Salma Abdelzaher: Writing – review & editing (equal). Tejas Guruswamy: Methodology (equal); Writing – review & editing (equal); Supervision (equal); Funding acquisition (equal). Tomas Polakovic: Methodology (equal); Writing – review & editing (equal); Funding acquisition (equal). Umeshkumar Patel: Methodology (equal); Writing – review & editing (equal); Funding acquisition (equal). Orlando Quaranta: Methodology (equal); Writing – review & editing (equal); Funding acquisition (equal). Thomas Cecil: Methodology (equal); Writing – review & editing (equal); Funding acquisition (equal). Clarence Chang: Methodology (equal); Writing – review & editing (equal); Funding acquisition (equal). Yu-Sheng Chen: Investigation (equal); Writing – review & editing (equal). Thomas H. Swift: Formal analysis (lead); Investigation (equal); Data curation (lead); Writing – review & editing (equal). Grayson M. Noah: Investigation (equal); Writing – review & editing (equal). Alberto Gomez-Saiz: Investigation (equal); Writing – review & editing (equal); Visualization (equal). John J. L. Morton: Investigation (equal); Writing – review & editing (equal); Visualization (equal). M. Fernando Gonzalez-Zalba: Investigation (equal); Writing – review & editing (equal); Visualization (equal). Antonino Miceli: Conceptualization (equal); Writing – original draft (equal); Writing – review & editing (equal); Supervision (equal); Project administration (equal); Funding acquisition (equal). Inna Partin-Vaisband: Conceptualization (equal); Writing – review & editing (equal); Supervision (equal); Project administration (equal); Funding acquisition (equal).
Data Availability
The data that support the findings of this study are available from the corresponding authors upon reasonable request.
References
- [1]M. Wittmer, “TiN and TaN as diffusion barriers in metallizations to silicon semiconductor devices,” Applied Physics Letters 36, 456–458 (1980).DOI
- [2]C. Lavoie, F. M. d’Heurle, C. Detavernier, and C. Cabral, Jr., “Towards implementation of a nickel silicide process for CMOS technologies,” Microelectronic Engineering 70, 144–157 (2003).DOI
- [3]T. Guruswamy, L. Gades, A. Miceli, U. Patel, and O. Quaranta, “Beamline spectroscopy of integrated circuits with hard X-ray transition edge sensors at the Advanced Photon Source,” IEEE Transactions on Applied Superconductivity 31, 1–5 (2021).DOI
- [4]M. R. Vissers, J. Gao, D. S. Wisbey, D. A. Hite, C. C. Tsuei, A. D. Corcoles, M. Steffen, and D. P. Pappas, “Low loss superconducting tantalum nitride coplanar waveguide resonators,” Applied Physics Letters 97, 232509 (2010).DOI
- [5]S.-P. Chiu, C. C. Tsuei, S.-S. Yeh, F.-C. Zhang, S. Kirchner, and J.-J. Lin, “Observation of triplet superconductivity in CoSi₂/TiSi₂ heterostructures,” Sci. Adv. 7, eabg6569 (2021).DOI
- [6]N. R. Groll, J. A. Klug, C. Cao, S. Altin, H. Claus, N. G. Becker, J. F. Zadzinski, M. J. Pellin, and T. Proslier, “Tunneling spectroscopy of superconducting MoN and NbTiN grown by atomic layer deposition,” Applied Physics Letters 104, 092602 (2014).DOI
- [7]S.-P. Chiu, C.-J. Wang, Y.-C. Lin, S.-T. Tu, S. K. Sahu, R.-T. Wang, C.-Y. Wu, S.-S. Yeh, S. Kirchner, and J.-J. Lin, “Electric and superconducting properties of CoSi₂ films on silicon — an unconventional superconductor with technological potential,” Chinese Journal of Physics 90, 348–363 (2024).DOI
- [8]T. H. Swift, F. Olivieri, G. Azipurua-Iraola, J. Kirkman, G. M. Noah, M. de Kruijf, F.-E. von Horstig, A. Gomez-Saiz, J. J. L. Morton, and M. F. Gonzalez-Zalba, “A superconductor in a deep sub-micron integrated circuit,” arXiv:2507.13202 (2025), 10.48550/arXiv.2507.13202.arxiv.org/abs/2507.13202
- [9]G. N. Gol’tsman, O. Okunev, G. Chulkova, A. Lipatov, A. Semenov, K. Smirnov, B. Voronov, A. Dzardanov, C. Williams, and R. Sobolewski, “Picosecond superconducting single-photon optical detector,” Applied Physics Letters 79, 705–707 (2001).DOI
- [10]A. E. Lita, A. J. Miller, and S. W. Nam, “Counting near-infrared single-photons with 95% efficiency,” Opt. Express 16, 3032–3040 (2008).pubmed.ncbi.nlm.nih.gov/18542389
- [11]C. M. Natarajan, M. G. Tanner, and R. H. Hadfield, “Superconducting nanowire single-photon detectors: physics and applications,” Supercond. Sci. Technol. 25, 063001 (2012).DOI
- [12]O. Quaranta, S. Marchetti, N. Martucciello, S. Pagano, M. Ejrnaes, R. Cristiano, and C. Nappi, “Superconductive three-terminal amplifier/discriminator,” IEEE Transactions on Applied Superconductivity 19, 367–370 (2009).DOI
- [13]A. N. McCaughan and K. K. Berggren, “A superconducting nanowire three-terminal electrothermal device,” Nano Letters 14, 5748–5753 (2014).
- [14]R. Baghdadi, J. P. Allmaras, B. A. Butters, A. E. Dane, S. Iqbal, A. N. McCaughan, E. A. Toomey, Q.-Y. Zhao, A. G. Kozorezov, and K. K. Berggren, “Multilayered heater nanocryotron: A superconducting-nanowire-based thermal switch,” Phys. Rev. Appl. 14, 054011 (2020).DOI
- [15]D. James, “High-k/metal gates in the 2010s,” in 25th Annual SEMI Advanced Semiconductor Manufacturing Conference (ASMC 2014) (2014) pp. 431–438.DOI
- [16]A. J. Kerman, J. K. W. Yang, R. J. Molnar, E. A. Dauler, and K. K. Berggren, “Electrothermal feedback in superconducting nanowire single-photon detectors,” Phys. Rev. B 79, 100509 (2009).DOI
- [17]A. J. Annunziata, O. Quaranta, D. F. Santavicca, A. Casaburi, L. Frunzio, M. Ejrnaes, M. J. Rooks, R. Cristiano, S. Pagano, A. Frydman, and D. E. Prober, “Reset dynamics and latching in niobium superconducting nanowire single-photon detectors,” J. Appl. Phys. 108, 084507 (2010).DOI
- [18]A. Dane, J. Allmaras, D. Zhu, M. Qnen, M. Colangelo, R. Baghdadi, N. Baškent, and K. K. Berggren, “Self-heating hotspots in superconducting nanowires cooled by phonon black-body radiation,” Nat. Commun. 13, 5429 (2022).DOI
- [19]M. Tinkham, J. U. Free, C. N. Lau, and N. Marković, “Hysteretic I–V curves of superconducting nanowires,” Phys. Rev. B 68, 134515 (2003).DOI
- [20]W. J. Skocpol, M. R. Beasley, and M. Tinkham, “Self-heating hotspots in superconducting thin-film microbridges,” J. Appl. Phys. 45, 4054–4066 (1974).DOI
- [21]G. Aizpurua-Iraola, T. H. Swift, F.-E. von Horstig, D. Prete, J. Kirkman, G. M. Noah, F. Olivieri, A. Gomez-Saiz, and M. F. Gonzalez-Zalba, “A superconducting phase transition single-electron transistor,” (2026), arXiv:2608.27045 [quant-ph].arxiv.org/abs/2608.27045
- [22]S. B. Kaplan, “Acoustic matching of superconducting films to substrates,” Journal of Low Temperature Physics 37, 343–365 (1979).DOI
- [23]E. T. Swartz and R. O. Pohl, “Thermal boundary resistance,” Rev. Mod. Phys. 61, 605–668 (1989).
- [24]T. H. Swift, Characterisation of superconductors and quantum dots in 22nm-node CMOS devices, Ph.D. thesis, University College London (2025).
- [25]J. Bardeen, G. Rickayzen, and L. Tewordt, “Theory of the thermal conductivity of superconductors,” Phys. Rev. 113, 982–994 (1959).DOI
- [26]A. V. Feshchenko, O.-P. Saira, J. T. Peltonen, and J. P. Pekola, “Thermal conductance of Nb thin films at sub-kelvin temperatures,” Sci. Rep. 7, 41728 (2017).DOI
- [27]A. J. Kerman, E. A. Dauler, J. K. W. Yang, K. M. Rosfjord, V. Anant, K. K. Berggren, G. N. Gol’tsman, and B. M. Voronov, “Constraint-limited detection efficiency of superconducting nanowire single-photon detectors,” Applied Physics Letters 90, 101110 (2007).DOI
- [28]D. Y. Vodolazov, “Single-photon detection by a dirty current-carrying superconducting strip based on the kinetic-equation approach,” Phys. Rev. Appl. 7, 034014 (2017).
- [30]A. Kardakova, M. Finkel, D. Morozov, V. Kovalyuk, P. An, C. Dunscombe, M. Tarkhov, P. Mauskopf, T. M. Klapwijk, and G. Goltsman, “The electron-phonon relaxation time in thin superconducting titanium nitride films,” Applied Physics Letters 103, 252602 (2013).DOI