Abstract

The spectral signatures of magnetic skyrmions under microwave field excitation are of fundamental interest and can be an asset for high frequency applications. These topological solitons can be tailored in multilayered thin films, but the experimental observation of their spin wave dynamics remains elusive, in particular due to large damping. Here, we study Pt/FeCoB/AlOx_x multilayers hosting dense and robust skyrmion lattices at room temperature with Gilbert damping of ∼0.02\sim 0.02. We use magnetic force microscopy to characterise their static magnetic phases and broadband ferromagnetic resonance to probe their high frequency response. Micromagnetic simulations reproduce the experiments with accuracy and allow us to identify distinct resonant modes detected in the skyrmion lattice phase. Low (<< 2 GHz) and intermediate frequency (2−82-8 GHz) modes involve excitations localised to skyrmion edges in conjunction with precession of the uniform background magnetisation, while a high frequency (>> 12 GHz) mode corresponds to in-phase skyrmion core precession emitting spin waves into uniform background with wavelengths in the 50–80 nm range commensurate with the lattice structure. These findings could be instrumental in the investigation of room temperature wave scattering and the implementation of novel microwave processing schemes in reconfigurable arrays of solitons.

The dynamic response of magnetic materials at microwave frequencies represents a rich field of research for its fundamental interest and applications in information processing. Linear excitations in the form of spin waves (SWs) underpin the field of magnonics, which describes the paradigm of transmitting and processing information with such waves[1, 2, 3]. SW-based devices may allow for fast and energy-efficient logic applications[4], and a growing number of proposals have shown potential uses for computing[5] and spectral analysis[6] by SW interference. Magnonic circuit elements such as transistors[7], diodes[8] and filters[9] have also been demonstrated in experiments based on the manipulation of dipole-dominated SWs with micrometer wavelengths. The generation and detection of shorter wavelength SWs, a prerequisite for miniaturization, is challenging, owing to the limitations of nanoscale fabrication. Recent studies have shown that short wavelength emission can be achieved by broadband antennae[10], grating effects[11, 12, 13] and spin torque[14].

In this light, nonuniform magnetic textures have been explored for generating and manipulating spin waves, and generally offer an alternate route to expand the range of useful phenomena for applications[15]. Such textures can appear spontaneously at the micro- and nano-scale in magnetic materials as a result of the competing interactions, namely, exchange, dipolar, and anisotropy. Magnetic textures like bubbles[16, 17], stripes[18, 19, 20], and vortices[21, 22] have been shown to exhibit a rich diversity of magnetisation dynamics. For example, it has been demonstrated that magnetic domain walls can serve as nanoscale waveguides[23, 24], while the cores of magnetic vortices can be used to generate omnidirectional dipole-exchange SWs with sub-100 nm wavelengths[25, 26].

Recently, topologically non-trivial chiral magnetic configurations called skyrmions have generated much interest owing to their robust and particle-like nature[27]. They can be stabilised at room temperature in thin films[28, 29] with perpendicular magnetic anisotropy (PMA) and interfacial Dzyaloshinskii-Moriya interaction (iDMI), which provides different handles for tuning the desired magnetic parameters, both statically and dynamically[30]. On one hand, their dc current-driven dynamics[31, 32] could be exploited for racetrack memory and logic devices[27], and on the other, their unique microwave response opens up the possibilities of skyrmion-based spin-torque oscillators[33], rf detectors[34], and reconfigurable magnonic crystals for microwave processing[35, 36, 37, 38]. Skyrmions exhibit a rich variety of eigenmodes[39, 40, 41, 42, 43], among which azimuthal bound states and breathing modes have been experimentally observed at low temperatures in bulk crystals[44, 45, 46], which have low damping parameters. Only very recently, resonant dynamics with specific spectroscopic signatures of thin-film multilayers hosting skyrmions has been evidenced[47, 48]. However, much remains to be explored and understood concerning their individual and collective resonant response to microwave excitations.

In this work, we report a study of the resonant dynamics of ultrathin film multilayers with perpendicular magnetic anisotropy, which host stable skyrmion lattices under ambient conditions with typical periods of 250 nm and skyrmion diameters of 100 nm, while exhibiting Gilbert damping in the range of α≃0.02\alpha\simeq0.02. By combining magnetic force microscopy (MFM) and ferromagnetic resonance (FMR) experiments with micromagnetic simulations, we can identify distinct SW modes associated with the skyrmion lattice phase. At low frequency (≲2\lesssim2 GHz), we observe a number of modes related to the precession of the uniform background state of individual layers close to or at the surfaces of the stack, along with eigenmodes localised to the skyrmion edges. At intermediate frequencies (2 – 8 GHz), the precession of the uniform background near the centre of the stack dominates the response. Similar modes were previously described and reported in bulk crystals[45, 46] and lately in thin films[47, 48]. Intriguingly, we also observe a well-defined mode at high frequency (>12> 12 GHz), which corresponds to the in-phase precession of the magnetisation within the skyrmion cores. The cores possess a distinct three-dimensional structure due to the competition between all the existing magnetic interactions in these multilayers, notably the interlayer dipolar effects[49]. Strikingly, this precession is accompanied by the emission of spin waves, with wavelengths in the range of 50 to 80 nm, into the uniformly magnetised background. These SWs interfere with those generated at neighbouring skyrmion cores, yielding a collective dynamical state governed by the subtle interplay between the skyrmion diameter, the wavelength of the emitted SWs, and the skyrmion lattice periodicity.

Results

Multilayer composition

The basic element of the multilayer film studied is the Pt(1.6)/Fe0.7_{0.7}Co0.1_{0.1}B0.2_{0.2}(1.2)/AlOx_x(1.0) trilayer (hereafter referred to as Pt/FeCoB/AlOx_x), where the figures in parentheses indicate the nominal film thickness in nm. This trilayer lacks inversion symmetry along the film thickness direction whereby the Dzyaloshinskii-Moriya interaction is promoted at the interfaces of the ferromagnetic FeCoB film with Pt (and possibly AlOx_x[50]). The trilayer is repeated 20 times to form our multilayer sample (see Methods), as shown in Figure 1(a). The choice of Fe-rich FeCoB and the aforementioned optimised thicknesses of Pt and FeCoB allow having sufficient DMI and PMA[51, 52, 53] to stabilise skyrmions, while limiting spin pumping effects which would otherwise lead to an increased damping coefficient[54]. We estimate by FMR a Gilbert damping constant of α=0.022\alpha= 0.022 and an inhomogeneous broadening of ∼18 mT (see Supplementary Figure 1) for our samples, which are relatively low for such multilayer systems[47, 54]. The overall magnetic volume is enhanced with the 20 repetitions of the trilayer, which not only increases the thermal stability of the skyrmions[28] but also provides a larger signal-to-noise ratio for inductive measurements.

Image not extracted

Figure 1. Static characterization of the magnetic phases. (a) Schematics of the sample stack. (b) The out-of-plane (OP) magnetisation curve on sweeping the field from negative to positive values. (c) The corresponding skyrmion density and apparent skyrmion diameter as a function of the field. The dashed red line indicates the possible extrapolation of the observed skyrmion density at higher positive field values in accordance with the OP hysteresis curve. The skyrmion diameter is extracted only for the field ranges where the skyrmion density is close to maximum, (see Methods). (d) Magnetic domain configurations of the sample: (i) randomly distributed skyrmions, (ii and vi) skyrmion lattice, (iii and v) skyrmion-stripe mix, and (iv) labyrinthine domains, measured by MFM as a function of OP magnetic field (corresponding to the values marked in (b)) swept from negative to positive values.

Static characterization

Figure 1(b) shows the out-of-plane hysteresis curve of the sample measured by alternating gradient field magnetometer (AGFM), which is characteristic of thin films hosting skyrmions. The quasi-static magnetisation configuration of the sample is probed by MFM using a low moment tip by sweeping the out-of-plane (OP) field from negative (−zz) to positive (+zz) saturation as illustrated in Figure 1(d). On decreasing the field from negative saturation, we observe nucleation of skyrmions with an average diameter around 100 nm (zone (i)), which develops into a dense lattice structure upon further reduction of the field (zone (ii)). In zone (iii) some of the skyrmions elongate and/or coalesce to form stripes leading to a mixture of skyrmions and stripe domains. At small positive fields, labyrinthine domains (zone (iv)) become energetically stable and, upon increasing the field further, lead to the formation of a dense skyrmion lattice once again (zone (vi)). From

the MFM images we extract the density of skyrmions as a function of the applied field μ0Hz\mu_0H_z and apparent skyrmion diameter for the ranges of magnetic field where the skyrmion density is close to maximum, as shown in Figure 1(c).

It is interesting to note that the observed skyrmion lattice is almost quasi periodic hexagonal (see Supplementary Figure 2) whereas more amorphous states were observed in previous studies[47, 48] in such kind of multilayered films, indicating only minor inhomogeneities and defects induced during the film growth in our samples. The skyrmion lattice phase is also remarkably stable at positive field, as shown by the constant skyrmion density of about 21 per square micron between 200 mT and 350 mT.

By using the period of the labyrinthine domain pattern in Figure 1(d)(iv) and the measured values of saturation magnetisation (Ms=1.2M_s = 1.2 MA/m) and uniaxial anisotropy (Ku=0.7K_u = 0.7 MJ/m3^3), we estimate the DMI to be D=1.2D = 1.2 mJ/m2^2 with an exchange constant of A=15A = 15 pJ/m for our sample (see Methods), which are in good agreement with direct experimental determination of these parameters in Pt/FeCoB/MgO stacks[55].

Dynamic characterization

The resonant dynamics of the sample was probed by broadband FMR using a coplanar waveguide [Figure 2(d)] and a vector network analyser (VNA). The dc out-of-plane field is swept from negative to positive values while the frequency of the in-plane ac field is scanned over a range of 0.1–20 GHz for each dc field step. The real and the imaginary parts of the transmission signal S21S_{21} are recorded and processed to remove a background signal that is independent of the dc field, which improves the contrast (see Methods and Supplementary Figure 3). The corresponding frequency versus field map is shown in Figure 2(a). In the saturated state, we observe the high intensity Kittel mode (KM) along with two additional low intensity secondary modes at higher field (see also Supplementary Figure 1). The latter are attributed to localised modes in the multilayer thickness that result from inhomogeneous interfacial couplings of our multilayer system[56]. In addition to the KM observed above saturation fields, three groups of modes with lower intensities appear when the magnetisation enters a non-uniform state. On ramping the field from negative saturation towards zero, the KM softens close to μ0Hz=−335\mu_0 H_z = -335 mT where skyrmions start to nucleate (see MFM images in Figure 1(d)). It then evolves into a mode with negative field dispersion (i.e., ∂f/∂∣Hz∣<0\partial f/\partial|H_z| < 0) as the skyrmion lattice grows denser, which we call the intermediate frequency mode (IFM). At this point, a weak amplitude mode also emerges at high frequency (>12> 12 GHz) which has a positive field dispersion (i.e., ∂f/∂∣Hz∣>0\partial f/\partial|H_z| > 0) denoted as the high frequency mode (HFM). The IFM and HFM fade away close to zero field, where the static magnetisation configuration consists of labyrinthine domains. While the IFM reappears as the field is increased towards positive values corresponding to a mixture of skyrmions and stripes, the HFM is visible only above 200 mT when the magnetisation profile consists of a dense skyrmion lattice network (see Figure 1(c)), and the IFM dispersion nearly flattens. We also notice that at the very same field a mode appears at low frequency (<2< 2 GHz) followed by another at even lower frequencies, which we refer to as low frequency modes (LFM). The HFM mode fades away at fields when the skyrmion lattice transforms into isolated skyrmions. The IFM continues beyond this point however with an abrupt change of slope until the magnetisation becomes uniform beyond 390 mT. The line cuts along fixed fields (−295 mT and 295 mT) and fixed frequencies (14 GHz and 4 GHz) are shown in Figure 2(b) and Figure 2(c) respectively. The modes at negative and positive fields are not symmetric but instead depend on the magnetic field history (see Supplementary Figure 4), as does the static magnetisation profile.

Broadband ferromagnetic resonance

Figure 2. Broadband ferromagnetic resonance. (a) Frequency-field dispersion map measured by VNA-FMR over a frequency range of 0.1 GHz to 20 GHz with the applied OP field swept from -500 mT to 500 mT. Apart from the Kittel mode (KM) above saturation, several distinct modes appear in the non-saturated state which are labelled as HFM: high frequency mode (f>12f > 12 GHz), IFM: intermediate frequency mode (f<8f < 8 GHz) and LFM: low frequency modes (f<2f < 2 GHz). (b) Line cuts for fixed OP field values: -295 mT and 295 mT. (c) Line cuts for fixed frequency values: 4 GHz and 14 GHz. (d) Schematic of the VNA-FMR setup.

Ferromagnetic resonance in the saturated state

Supplementary Figure 1. Supplementary Figure 1 | Ferromagnetic resonance in the saturated state. (a) Evolution of the resonance field as a function of the angle θH\theta_{\mathrm{H}} between the applied field and the film plane, determined by cavity-FMR at 9.725 GHz. The continuous line is the theoretical expectation using the values of gyromagnetic ratio and total uniaxial anisotropy field extracted from out-of-plane (OP) and in-plane (IP) configurations given in the text. (b) Corresponding dependence of the FMR linewidth on θH\theta_{\mathrm{H}}. The dashed line is a guide to the eye. Inset: spectrum measured in the OP configuration. The resonance field of the uniform Kittel mode is 691.2 mT, additional modes are observed at 718.3 mT and 737.2 mT. (c) Dependence of the in-plane FMR linewidth on frequency measured by broadband FMR. The red line is the linear fit yielding the damping parameter and the inhomogeneous contribution.

Six-panel VNA-FMR data processing maps

Supplementary Figure 3. VNA-FMR data processing. (a) Intensity map of the 30-cycle averaged transmission signal S21S_{21} in the field–frequency coordinates, the field being swept upwards. (b) Map of the S21S_{21} data processed using the derivative method. (c) Map of the S21S_{21} data processed using the derivative method followed by a frequency differentiation. (d–f) same as (a–c) for the magnetic field being swept downwards. In addition to the narrow signals ascribed to ferromagnetic resonances in the multilayer sample, there is a very broad background signal coming from the measurement cell which is symmetric between negative and positive field values, as can be seen from the distorted ”V” shape in panels (b) and (e), and independent of the sweep direction – in strong contrast with the resonances originating from the multilayer sample (see also Supplementary Figure 4). The frequency differentiation attenuates the broad background signal and improves the signal-to-noise ratio of the narrow resonances from the sample, as seen from panels (c) and (f).

Hysteretic character of the FMR modes

Supplementary Figure 4. Hysteretic character of the FMR modes. (a) OP magnetisation curves determined using alternating gradient force magnetometry by sweeping the field up and down. (b) Corresponding dependence of FMR modes determined by broadband VNA-FMR.

Micromagnetic simulations

We performed simulations with the finite-difference micromagnetic code Mumax3[57] in order to gain better insight into the static and dynamic properties of our sample (see Methods). We modelled the full 20-layer repetition of the Pt/FeCoB/AlOx_x trilayer (with periodic boundary conditions in the film plane) in order to account for dipolar effects as accurately as possible, since it is known that the skyrmion core deviates from the usual tubular structure to complex three-dimensional configurations due to inhomogeneous dipolar fields along the multilayer thickness[49]. Figure 3(a) and Figure 3(b) show the simulated hysteresis loop and the skyrmion density and apparent diameter variation as a function of the OP field swept from negative to positive values. The MFM images calculated from the simulated magnetisation profiles (see Methods) are shown in Figure 3(c). The field evolution of the simulated static characteristics presented in Figure 3(a)–(Figure 3c) is found to be in good agreement with the experiments.

Micromagnetic simulations of equilibrium magnetic configuration

Figure 3. Micromagnetic simulations of equilibrium magnetic configuration. (a) Simulated magnetisation curve, (b) skyrmion density and diameter evolution and (c) the corresponding simulated MFM images for the OP field swept from negative to positive values. The grey shaded area in (b) results from uncertainties in determining the skyrmion diameter, as discussed in the Methods section. (d) mzm_z contours and (e) in-plane components of the magnetisation texture of a single skyrmion in the lattice phase at 285 mT. (f) Topological charge density QQ per layer 285 mT. (g) Magnetic configuration of layer 12 at 285 mT.

A striking feature of the labyrinthine domain and skyrmion structures found is that their micromagnetic configuration exhibits strong variations along the multilayer thickness direction. An example of such complex structures is shown in Figure 3(d), where the mzm_z component is shown for a single skyrmion core in the lattice phase at μ0Hz=285\mu_0 H_z = 285 mT. The figure shows the contours for mz=0.9m_z = 0.9 (red), mz=0m_z = 0 (yellow), and mz=−0.9m_z = -0.9 (blue) as surfaces where cubic interpolation has been used across the nonmagnetic layers. We note that the skyrmion core, in particular the region of reversed magnetisation mz≤−0.9m_z \leq-0.9, does not extend across the entire thickness of the multilayer. Recall that the FeCoB layers are only coupled together through dipolar interactions, which are sufficiently large to maintain an alignment of the core centre but too weak to promote a coherent magnetisation profile across the different layers. We can also observe that the magnetisation in the uppermost layers at the core centre is not reversed at all, but slightly tilted away from the film normal as indicated by the presence of the inverted cone. The in-plane components of the magnetic texture shown in Figure 3(d) are presented in Figure 3(e). Here, each cube represents the magnetic state of a finite-difference cell, where the colour represents the orientation of the magnetisation in the cell. In order to highlight the role of the in-plane components to complement the data shown in Figure 3(d), the relative size and opacity of each cube is scaled with the function 1−mz21 - m_z^2; this renders the regions of the uniform background and the reversed magnetisation transparent. A clear skyrmion profile can be seen for the nine bottom layers, where the same left-handed (i.e. counterclockwise) Néel chirality is found in each layer. In layers 10 to 14, on the other hand, the in-plane component of the magnetisation at the skyrmion boundary becomes more uniform and does not exhibit the same winding as in the bottom half of the stack. This means that the reversed domain structure is non-topological. A skyrmion profile reappears in layers 15, 16 and 17 but with a reversed chirality, where the in-plane magnetisation components of the right-handed (i.e. clockwise) Néel structure are rotated by 180 degrees in the plane with respect to their left-handed counterparts. Finally in layers 18 to 20, we observe another type of non-topological texture where the core magnetisation is closely aligned with the background magnetisation, which corresponds to the inverted cone at the top of the stack in Figure 3(d). Figure 3(f) shows the variation of the topological charge density per layer as a function of the layer number, which shows that a similar thickness dependence is observed across the skyrmion lattice. The skyrmions in the bottom half of the stack remain topological, while the top half comprises largely non-topological bubbles. Finally, Figure 3(g) illustrates the magnetic configuration of layer 12 across the entire region simulated, where we can observe that the mainly uniformly-magnetised regions of the magnetic bubble walls can vary greatly from one bubble to the next, with no discernible spatial order. We have verified that these features persist for finite difference cell sizes down to ∼2\sim2 nm, which indicates that the complex magnetisation structure does not arise from discretization effects (see Supplementary Figure 5).

Mesh size dependence of static states, showing panels a–o

Supplementary Figure 5. Mesh size dependence of static states. The simulated static properties, as discussed in Figure 3 of the main text, are shown for three different discretisation schemes for 1 µm of the simulated geometry: 128 (as discussed in the main text), 256, and 512 cells. (a–c), Hysteresis loops. (d–f), Density plots of the topological charge density per layer as a function of perpendicular applied field BzB_z. (g–i), In-plane components of the magnetisation configuration for a skyrmion at Bz=285B_z = 285 mT. (j–l), Topological charge density as a function of layer number at Bz=285B_z = 285 mT. (m–o), Magnetisation configuration of layer 12 at Bz=285B_z = 285 mT, where the dashed boxes indicate the state shown in (g–i), respectively.

We next discuss the dynamical response of the system, where the frequency-dependent susceptibility is computed under different applied fields as in Figure 2(a) (see Methods). The simulated susceptibility map is shown in Figure 4(a), which is determined from response of the static configurations computed in Figure 3 to sinusoidal in-plane fields in the frequency range of 0.1 to 20 GHz.

Micromagnetic simulations of the dynamic response

Figure 4. Micromagnetic simulations of the dynamic response. (a) FMR spectra simulated by calculating the frequency-dependent susceptibility of multilayer to uniform excitation fields. (b) Imaginary part of the magnetic susceptibility at 285 mT (indicated by a dashed line in (a)), showing three LFM (0.94, 1.50, and 1.92 GHz), two IFM (3.90 and 4.24 GHz) and one HFM (15.10 GHz). (c) Thickness-resolved susceptibility at 285 mT. (d, e, f) Three-dimensional view of the magnetic response ⟨δmx⟩\langle\delta m_x\rangle for (d) LFM, (e) IFM, and (f) HFM. (g, h, i) Two-dimensional view of the magnetic response ⟨δmx⟩\langle\delta m_x\rangle in layer 10 of the modes in (d,e,f) for (g) LFM, (h) IFM, and (i) IFM.

The Kittel mode (KM) is easily identified for the uniform state for fields above the saturation field. In the regime in which the magnetisation is nonuniform, −330<μ0Hz<365-330 < \mu_0 H_z < 365 mT, three distinct types of modes can be identified, as illustrated by the line cut at 285 mT shown in Figure 4(b). As in experiments, the KM transforms into a negative field dispersion mode, an intermediate frequency mode (IFM), at fields where skyrmion nucleation begins. The IFM dispersion is rather rugged on the negative field side, where the skyrmion density rapidly evolves with field, and a faint splitting of IFM is seen around −260-260 mT. The IFM is asymmetric with respect to zero field and exhibits smoother variations on the positive field side. Similar to the negative field side, another branch of the IFM is seen for positive fields appearing at around 200 mT, which is relatively flat around 4 GHz in the range of positive magnetic fields 240≤μ0Hz≤345240 \le\mu_0 H_z \le345 mT, where a dense skyrmion lattice is stable. It then merges to a single IFM and then varies sharply until saturation. Several low frequency modes (LFMs), comprising several closely spaced branches in the frequency range of 0.5<f<2.50.5 < f < 2.5 GHz, extend over the entire magnetic field range in which the magnetisation is non-uniform. Finally, a high frequency mode (HFM) is also observed above 10 GHz with a positive field dispersion. It exhibits a sawtooth-like variation at negative fields and a smoother variation for positive fields. It is attenuated in the field range where magnetisation profile consists of randomly oriented stripes (region (iv) in Figure 3). The simulated susceptibility map reproduces well the three families of modes observed experimentally in the non-saturated state and gives good quantitative agreement for the mode frequencies. Note that in experiments, the LFM branches could not be resolved for the negative field side in the S21S_{21} transmission data of Figure 2(a) (as opposed to the S11S_{11} and S22S_{22} reflection data, presented in Supplementary Figure 6). It is because these modes have a nearly flat frequency–field dispersion, and hence get diluted in the signal processing which is necessary to remove the field independent offset. Only two of the LFM branches become resolvable when they acquire a certain slope on the positive field side, where the skyrmion density is constant and the skyrmion size strongly varies with the field.

The spatial profiles of the excited modes are found by driving the system at the mode frequencies identified in Figure 4(a) and by recording the resonant response. In Figure 4(b), we present the frequency response for μ0Hz=285\mu_0 H_z = 285 mT at which the equilibrium ground state is a skyrmion lattice, where we can identify well-defined peaks corresponding to the LFM, IFM, and HFM. Figure 4(c) gives layer-resolved susceptibility whose sum over all layers results in the curve in Figure 4(b). For the LFM, we observe that the peaks in Figure 4(b) correspond to two kinds of resonances. For LFM 1 at f=0.94f = 0.94 GHz, the primary response arises from the central part of the stack in layers 13 and 14, and also from the top of the stack in layer 20. A similar behaviour is seen for LFM 2 at 1.50 GHz, where layers 1 and 19, close to the stack surfaces, resonate along with the central part of the multilayer, as with LFM 3 at 1.92 GHz, where a strong response is seen in layers 2 and 18. This trend continues as the frequency increases, where successive layers farther away from the surfaces exhibit local resonances in conjunction with the central part. These mode profiles are visualised in Figure 4(d), where we show the resonant fluctuations in the xx component of the magnetisation, ⟨δmx⟩\langle\delta m_x\rangle (see Methods). Blue regions give the main response to the susceptibility, while the sum of equally intense blue and red regions cancel each other out. Similarly to Figure 3(e), the opacity of the cells increase with the strength of the response in order to provide a clearer picture of their spatial profiles. LFM 1 mainly corresponds to the uniform precession of the background magnetisation at the top of the multilayer stack, while the skyrmion edges are also excited in the central part of the stack with a small overall contribution to the susceptibility. This can be seen more clearly in Figure 3(g), where the fluctuations are shown for layer 10. For LFM 2 and LFM 3, a similar behaviour is seen where individual layers precess uniformly close to the surfaces, while excitations in the central part are localised to skyrmion edges.

For the IFM, two broad resonances are identified at μ0Hz=285\mu_0 H_z = 285 mT and correspond to excitations that are mainly localised to the central part of the multilayer [Figure 4(c,Figure 4e)]. The main contribution comes from the uniform precession of the background magnetisation between the skyrmion cores, i.e., the inter-skyrmion region which is aligned parallel to the applied field, which can been seen from the predominantly blue regions in Figure 4(h) that appear outside the cores. In addition, some SW channelling is also observed at the skyrmion edges, as shown by alternating red and blue patches encircling the skyrmions.

The HFM involves the in-phase precession of the reversed magnetisation within the skyrmion cores and extends across most of the multilayer [Figure 4(c,Figure 4f)], with much of the power concentrated in the central part of the stack. The coherence of the precession can be seen in Figure 4(i) by the uniform blue zones of ⟨δmx⟩\langle\delta m_x \rangle within the mz=0m_z = 0 contours denoted by the continuous black circles. Moreover, this precession results in the generation of short wavelength SWs in the inter-skyrmion region, which are almost as intense as the core precession. However, only the volume occupied by the skyrmion cores provides a coherent response to the susceptibility for the HFM, which explains its much weaker intensity compared to the IFM and KM.

These features are also present at other applied field values at which the equilibrium state comprises nonuniform magnetisation. Supplementary Figure 7 shows an analogous behaviour at μ0Hz=−285\mu_0 H_z = -285 mT, where the lattice possesses a lower skyrmion density with deformed core profiles. At μ0Hz=140\mu_0 H_z = 140 mT where the equilibrium state comprises labyrinthine domains, only the LFM and IFM are present, which further highlights the link between the HFM and the precessing skyrmion cores (Supplementary Figure S8). At zero field, the equilibrium state comprises a mixture of bubbles and elongated stripes in which no clear background orientation can be defined. Here, LFM persist while the IFM and HFM are absent. Instead, we can observe the existence of cavity modes that represent confined spin waves (Supplementary Figure 9).

Micromagnetic simulations of the dynamic response

Supplementary Figure 7. Micromagnetic simulations of the dynamic response at μ0Hz=−285\mu_0 H_z = -285 mT. (a) Field-dependent susceptibility map, reproduced from Figure 4(a). (b) Imaginary part of the magnetic susceptibility at -285 mT, showing six LFM (0.6, 1.06, 1.16, 1.4, 1.6, and 2.08 GHz), two IFM (2.92 and 3.1 GHz) and one HFM (13.52 GHz). (c) Thickness-resolved susceptibility at -285 mT. (d, f, g) Three-dimensional view of the magnetic response ⟨δmx⟩\langle\delta m_x\rangle for (d) LFM, (f) IFM, and (g) HFM. (e, h, i) Two-dimensional view of the magnetic response ⟨δmx⟩\langle\delta m_x\rangle in layer 10 of the modes in (d,f,g) for (e) LFM, (h) IFM, and (i) IFM, respectively.

Micromagnetic simulations of the dynamic response

Figure S8. Micromagnetic simulations of the dynamic response at μ0Hz=140\mu_{0}H_{z}=140 mT. (a) Field-dependent susceptibility map, reproduced from Figure 4(a). (b) Imaginary part of the magnetic susceptibility at 140 mT, showing five LFM (1.02, 1.2, 1.36, 1.96, and 3 GHz) and one IFM (6.54 GHz). No HFM is observed because no skyrmions are present. (c) Thickness-resolved susceptibility at 140 mT. (d, e) Three-dimensional view of the magnetic response ⟨δmx⟩\langle\delta m_{x}\rangle for (d) LFM and (e) IFM. (f, g) Two-dimensional view of the magnetic response ⟨δmx⟩\langle\delta m_{x}\rangle in layer 10 of the modes in (d,e) for (f) LFM and (g) IFM, respectively.

Micromagnetic simulations of the dynamic response

Supplementary Figure 9. Micromagnetic simulations of the dynamic response at μ0Hz=0\mu_{0}H_{z} = 0 mT. (a) Field-dependent susceptibility map, reproduced from Figure 4(a). (b) Imaginary part of the magnetic susceptibility at 0 mT, showing four LFM (0.7, 1.06, 1.56, and 2.1 GHz) and three cavity modes (CM) (8.02, 10.62, and 13.14 GHz), where the latter represent spin wave excitations confined within the bubble or elongated stripe domains. (c) Thickness-resolved susceptibility at 0 mT. (d, e) Three-dimensional view of the magnetic response ⟨δmx⟩\langle\delta m_x\rangle for (d) LFM and (e) CM. (f, g) Two-dimensional view of the magnetic response ⟨δmx⟩\langle\delta m_x\rangle in layer 10 of the modes in (d,e) for (f) LFM and (g) CM, respectively.

Spin wave emission from the high frequency mode

The short wavelength SWs associated with the HFM cannot be excited directly with the uniform driving fields used in FMR, so their presence indicates the skyrmion cores act as nanoscale transducers that convert a spatially-uniform drive into a spatially-nonuniform excitation. To obtain deeper insight into this process, we focus on the HFM in the simulation data at two values of the applied fields, 300 and 364 mT, as presented in Figure 5. The equilibrium state at 300 mT comprises a skyrmion lattice, with a skyrmion density of 20 μm−2\mu\mathrm{m}^{-2} and an average core-to-core distance of L=262L = 262 nm, while only one metastable skyrmion is present at 364 mT within the same area. The skyrmion diameters are roughly equivalent at these field values, which are 95 and 94 nm, respectively. The susceptibility at these two fields, shown in Figure 5(a) for the range of 12–17 GHz, display a clear resonance peak around 15.5 GHz, which is over an order of magnitude larger at 300 mT than at 364 mT due to the difference in the skyrmion density.

Emission and interference of spin waves in skyrmion lattice

Figure 5. Emission and interference of spin waves in skyrmion lattice. (a) Simulated susceptibility curves at 300 mT and 364 mT with the dynamic magnetisation profiles ⟨δmx⟩\langle\delta m_x\rangle in (b) and (c) of layer 10, respectively, corresponding to the resonance at 15.5 GHz. Cross-sections of ⟨δmx⟩\langle\delta m_x\rangle marked by dotted lines in (b) and (c) are also shown respectively in panels (d) and (e), highlighting the in-phase skyrmions core precession (in blue) and spin wave emission in the surrounding medium (alternate blue and red zones) (f,g) Power spectral density (PSD) of the layer averaged spatial discrete Fourier transform of the dynamic magnetisation profiles indicating the average kSWk_{\mathrm{SW}}-vector of the emitted SWs at 300 mT and 364 mT respectively. At 300 mT, the skyrmion lattice parameter can also be deduced from the k=24k = 24 μm−1\mu\mathrm{m}^{-1} periodic pattern seen in the spatial Fourier transform.

At both field values, the coherent precession of the reversed magnetisation within the skyrmion cores emit spin waves into the ferromagnetic background. Their wavelengths are similar at both fields and are estimated from the ⟨δmx⟩\langle\delta m_x \rangle profiles in layer 10 shown in Figure 5(b) and Figure 5(c), yielding λ≃60\lambda\simeq60 nm and λ≃54\lambda\simeq54 nm at μ0Hz=300\mu_0 H_z = 300 mT and μ0Hz=364\mu_0 H_z = 364 mT, respectively. Despite the strong variations in the static core profile across the multilayer thickness, the emitted spin waves are remarkably coherent across the thickness. This can be seen in Figure 5(d) for 300 mT and Figure 5(e) for 364 mT where coherent wavefronts, driven in the central part of the multilayer at which the core diameter is greatest, extend across much of the multilayer thickness. The left inset in Figure 5(d,Figure 5e) indicate the number of topological charges per layer, which shows that the spin wave emission is just as effective for the topological bubbles residing primarily in the bottom of the stack as for the non-topological bubbles residing primarily in the top.

The overall coherence of these spin wave excitations can also be seen from the layer-averaged spatial discrete Fourier transform of the dynamical magnetisation shown in Figure 5(b,Figure 5c). These Fourier maps, shown in Figure 5(f,Figure 5g), display a ring pattern with wave vectors 100 ≲kSW μm−1\lesssim k_{\mathrm{SW}} \ \mu\mathrm{m}^{-1} corresponding to wavelengths 40<λ<6040 < \lambda< 60 nm. At 300 mT, the pattern in the Fourier transformed data also manifests the periodic structure of the skyrmion lattice, from which the lattice periodicity can be estimated as shown in Figure 5(f), using 2π/k=2622\pi/k = 262 nm, where k=24k = 24 μm−1\mu\mathrm{m}^{-1}.

The spin wave dynamics can be understood from the linearised equations of motion for the dynamic magnetisation δm\delta\mathbf{m}, ∂tδm=−∣γ0∣(δm×Heff,0+m0×δHeff)\partial_t \delta\mathbf{m} = -|\gamma_0|(\delta\mathbf{m} \times\mathbf{H}_{\mathrm{eff},0} + \mathbf{m}_0 \times\delta\mathbf{H}_{\mathrm{eff}}), where m0\mathbf{m}_0 is the static magnetisation configuration and Heff,0\mathbf{H}_{\mathrm{eff},0} is the static effective (internal) field associated with m0\mathbf{m}_0, while δHeff\delta\mathbf{H}_{\mathrm{eff}} is the dynamic effective (internal) field associated with δm\delta\mathbf{m}. The full 3D structure of the core and the surrounding configuration determines the spatial profile of the static internal field and the localisation of the mode. The average value of this static internal field Heff,0(r)\mathbf{H}_{\mathrm{eff},0}(\mathbf{r}) inside the skyrmion core can be extracted from micromagnetic simulations and is about ∼200\sim200 mT, which leads to resonances at 5.8 GHz without any confinement effects. To this, one needs to add the dynamic dipolar and exchange contributions δHeff(r,t)\delta\mathbf{H}_{\mathrm{eff}}(\mathbf{r},t) due to the localisation of magnetisation dynamics in a volume of ∼100×100×50\sim100 \times100 \times50 nm3^3, which increases the resonant frequency to about 15 GHz (see Supplementary Note 2). Similarly, we can estimate the wavelength of the emitted SWs by using the dispersion relation of forward-volume SWs in the inter-skyrmion region. At 300 mT, the average internal field in this region is around 110 mT, which results in a wavelength of 60 nm at 15.5 GHz, a group velocity of 960 m/s and an attenuation length of 490 nm (see Supplementary Figure 10). These estimations are in good agreement with the SW characteristics observed in Figure 5.

Internal field map and spin wave dispersion

Supplementary Figure 10. Internal field and spin wave dispersion. (a) Map of the internal field extracted from micromagnetic simulations at 300 mT in layer 12. Values are given in units of mT. (b) Dispersion relation of forward-volume SWs calculated using Eq. (4) for a uniform internal field of 110 mT. (c) Corresponding group velocity. The dashed lines in panels (b) and (c) highlight the SWs excited at 15.5 GHz, whose wavelength and group velocity are respectively found to be λ=59.8\lambda= 59.8 nm and Vg=960V_g = 960 m/s.

The difference between the mode profiles shown in Figure 5(b) and Figure 5(c) is due to interference effects. At low skyrmion densities, the SW emitted at one core attenuates before reaching another, resulting in the familiar concentric ripples around each excitation source. At higher skyrmion densities, on the other hand, the inter-skyrmion distance is smaller than the attenuation length and interference patterns can arise. The cores can emit SWs in a broad spectral range, which depends on the excitation frequency and the skyrmion size (see Supplementary Figure S11). As such, the overall collective behavior is governed by a subtle interplay between the characteristic length scales of the system. The skyrmion diameter, which varies with the applied magnetic field, determines the precession frequency of the core thereby the wavelength of the emitted SWs, whereas constructive or destructive SW interference patterns are determined by the commensurability of SW wavelength and lattice parameters.

Frequency dependence of the SW interference pattern

Figure S11. Frequency dependence of the SW interference pattern. Dynamic magnetisation excited in layer 10 at 300 mT (top) and 364 mT (bottom) by an in-plane microwave field of frequency ranging from 10 GHz to 18 GHz, and associated layer averaged spatial FFT. The most efficient frequency to drive the core precession corresponds to the resonance frequency of 15.5 GHz. When using a lower or higher frequency to drive the system, its overall response has a lower amplitude. In addition, following the trend of the dispersion relation shown in Supplementary Figure 10, the wave vector of the emitted SWs increases with the excitation frequency of the skyrmion core, as seen from the FFT maps. As a result, the resulting interference patterns also change, in a way that depends on the skyrmion lattice, as shown by the comparison between 300 mT and 364 mT. More generally, the interference patterns depend on the characteristic lengths of the system, which can be tuned by the applied OP field. Both the density and the diameter of the skyrmions indeed depend on the field (see Figure 3(b) of the main text), which determines the travel length of the SWs between the boundaries of neighbouring skyrmions.

Discussion

SW emission related to the HFM can have advantages over other reported methods of sub-100 nm wavelength generation. For example, magnetic vortex cores, which can act as SW emitters, require confined geometries such as dots for their existence and do not spontaneously form lattice structures in continuous films, which precludes the appearance of SW interference phenomena seen here. The precession frequency of the skyrmions in our samples is also above the FMR gap of the surrounding domain background and hence SWs can be excited at this frequency in the same medium, unlike in other hybrid structures such as Pt/Co/YIG[58]. Moreover, the SWs generated in PMA materials are forward-volume SWs, which propagate isotropically[59] compared to backward-volume and Damon-Eshbach modes in in-plane magnetised systems, while maintaining high group velocities.

An interesting analogy of our skyrmion lattice as SW emitters can be made with arrays of spin-torque nano-oscillators, which can generate propagating SWs and get synchronised via them[60]. These structures have been proposed for implementing unconventional computing schemes[5]. We have shown here that SWs can be emitted in the uniform background by the skyrmion dynamics, but one also expects that in return, SWs can influence the skyrmion dynamics[39], which could enlarge the processing capabilities of this type of devices.

Our study also paves the way toward creating reconfigurable magnonic crystals, since the skyrmion lattices we observe are quasi-periodic and dynamically tunable[37]. We can get a glimpse of the role of this lattice in the observation of SW interference patterns in the simulated HFM. However, the properties of the skyrmion lattice as a magnonic crystal also needs to be explored using broadband propagating SW spectroscopy[10] or advanced SW imaging methods[9, 25]. Lastly, our system could serve as a platform to study magnon-skyrmion scattering[39], emergent magnon motifs[61], or chiral magnonic edge states[62].

Methods

Experimental details

Ta(10)/Pt(8)/[FeCoB(1.2)/AlOx_x(1.0)/Pt(1.6)]19_{19}/FeCoB(1.2)/AlOx_x(1.0)/Pt(3) multilayer stacks (where FeCoB ≡\equiv Fe70_{70}Co10_{10}B20_{20}, and thicknesses given in nm) were deposited by dc magnetron sputtering at room temperature on thermally-oxidised silicon substrates, under Ar gas flow at a pressure of 0.25 Pa. The base pressure of the sputtering equipment was 5×10−65 \times10^{-6} Pa. Magnetisation cycles were measured by alternating gradient force magnetometry on 3×33 \times3 mm2^2 films. MFM images were obtained at room temperature and ambient pressure using a double-pass lift mode, detecting the phase shift (MFM signal) of the second pass after a topographic measurement. The employed low moment tips were home made[49]. Small permanent magnets with tunable gap and calibrated values of field were used to bias the samples while imaging them. VNA-FMR was conducted on 2×4 mm22 \times4\ \mathrm{mm}^{2} films facing the 50 μm50\ \mu\mathrm{m} wide central conductor of a 50 Ω50\ \Omega matched coplanar waveguide. The OP magnetic field was ramped up and down between −550 mT-550\ \mathrm{mT} and +550 mT+550\ \mathrm{mT}. For each of the 400 field steps, the VNA frequency was swept from 0.1 GHz0.1\ \mathrm{GHz} to 20 GHz20\ \mathrm{GHz} with a number of points set to 1491 and a sweep time of 45 s. To improve the signal to noise ratio, the data were averaged over 30 magnetic field cycles. To remove the field independent background and normalise the transmission signal data S21S_{21}, we calculate dDS21\mathrm{d}_{\mathrm{D}}S_{21} using the derivative divide method [63]. To increase the contrast further, we apply an additional frequency differentiation, and plot the imaginary part of the obtained quantity in Figure 2(a).

Extraction of magnetic parameters

The magnetisation of the studied multilayers was determined by SQUID magnetometry. The 1.2 nm thick FeCoB is found to have a saturation magnetisation Ms=1.20±0.1 MA/mM_{\mathrm{s}} = 1.20 \pm0.1\ \mathrm{MA/m}. Using angle dependent cavity-FMR, the gyromagnetic ratio γ0/(2π)=28.75±0.10 GHz/T\gamma_{0}/(2\pi) = 28.75 \pm0.10\ \mathrm{GHz/T} and the total uniaxial anisotropy field including demagnetising and PMA contributions μ0(Ms−Hk)=354.7±0.5 mT\mu_{0}(M_{\mathrm{s}} - H_{\mathrm{k}}) = 354.7 \pm0.5\ \mathrm{mT} are determined (see Supplementary Note 1). In the case of uniaxial anisotropy μ0Hk=2Ku/Ms\mu_{0}H_{\mathrm{k}} = 2K_{\mathrm{u}}/M_{\mathrm{s}}, hence Ku=0.69±0.11 MJ/m3K_{\mathrm{u}} = 0.69 \pm0.11\ \mathrm{MJ/m}^{3}. By assuming Ms=1.2 MA/mM_{\mathrm{s}} = 1.2\ \mathrm{MA/m} and Ku=0.7 MJ/m3K_{\mathrm{u}} = 0.7\ \mathrm{MJ/m}^{3}, the DMI and exchange parameters were iteratively determined by adjusting the period of the simulated labyrinthine domains to the one (≃170 nm\simeq170\ \mathrm{nm}) observed by MFM at remanence[49]. We find the DMI constant to be D=1.2 mJ/m2D = 1.2\ \mathrm{mJ/m}^{2} for an exchange constant A=15 pJ/mA = 15\ \mathrm{pJ/m}.

Determination of skyrmion diameter

From the MFM measurements of the quasi static magnetic configuration as a function of the applied field, we extract skyrmion density by using a MATLAB program which uses binarisation. However, as the image resolution is not good enough to estimate the skyrmion diameters directly from the MFM images (which would anyway require to know the transfer function of the tip[64], and might be complicated by the influence of the tip’s stray field), we extract the apparent skyrmion diameters (2Rsk2R_{\mathrm{sk}}) indirectly, for the field values where the skyrmion density (dskd_{\mathrm{sk}}) is close to maximum, using the out-of-plane experimental magnetisation curve: Rsk=(1−mz)/(2πdsk)R_{\mathrm{sk}} = \sqrt{(1-m_{z})/(2\pi d_{\mathrm{sk}})}. In Figure 1(c) the error bars constitute the errors on the skyrmion density (proportional to the density and inversely proportional to the image size: ∼8%\sim8\%) and magnetic field values to account for the slight misalignment of the magnetic pole and the magnetic tip in the MFM setup (10%). In the case of simulated MFM images, we used the same MATLAB program that binarises the simulated MFM images, detects and finds the diameters of all the skyrmions, and calculates the mean and the standard deviation. For the simulations, we also compared the skyrmion diameter i/ calculated by the program and ii/ estimated from skyrmion density and mzm_z curve as a function of field when the skyrmion density is close to maximum. The small difference in the skyrmion diameters for the two methods lies within the standard deviation of the former method, indicated by the shaded area in grey in Figure 3(b).

Micromagnetic simulations

Simulations were carried out with the open-source finite-difference micromagnetics code Mumax3[57]. We used values of Ms=1.3375 MA/mM_{\mathrm{s}} = 1.3375\ \mathrm{MA/m} and Ku=0.9 MJ/m3K_{\mathrm{u}} = 0.9\ \mathrm{MJ/m}^{3}, which are slightly larger than the experimentally-determined values but were chosen to reproduce quantitatively the mode frequencies (see Supplementary Figure 12). The geometry consists of a rectangular slab of volume 1 μm×1 μm×72 nm1\ \mu\mathrm{m} \times1\ \mu\mathrm{m} \times72\ \mathrm{nm} discretised using 128×128×60128 \times128 \times60 rectangular cells for the susceptibility calculations and a volume of 2 μm×2 μm×72 nm2\ \mu\mathrm{m} \times2\ \mu\mathrm{m} \times72\ \mathrm{nm} with 256×256×60256 \times256 \times60 cells for the quasi-static hysteresis loop calculations. The simulated stack consists of 20 ferromagnetic layers with thickness 1.2 nm separated by 2.4 nm empty spacers, which accurately mimics the experimental stack, in which the total thickness of non-magnetic Pt and AlOx_x layers separating adjacent FeCoB layers is 2.6 nm. Periodic boundary conditions are used in xx and yy directions in the film plane. The code performs a numerical time integration of the Landau-Lifshitz-Gilbert equation for the magnetisation dynamics,

Optimisation of magnetic parameters used in micromagnetic simulations

Supplementary Figure 12. Optimisation of magnetic parameters used in micromagnetic simulations. Simulated imaginary part of the dynamic susceptibility, Im⁡[χ(f)]\operatorname{Im}[\chi(f)], as a function of applied perpendicular field, μ0Hz\mu_{0}H_{z}, for deviations from experimentally-determined values of the micromagnetic parameters, (a) Ms,0=1.2M_{s,0}=1.2 MA/m, A0=15A_{0}=15 pJ/m, Ku,0=0.70K_{u,0}=0.70 MJ/m3^{3}, and D0=1.2D_{0}=1.2 mJ/m2^{2}. (b) Ku=Ku,0+0.04K_{u}=K_{u,0}+0.04 MJ/m3^{3}, (c) Ku=Ku,0−0.04K_{u}=K_{u,0}-0.04 MJ/m3^{3}, (d) A=A0+5A=A_{0}+5 pJ/m, (e) A=A0−5A=A_{0}-5 pJ/m, (f) D=D0+0.03D=D_{0}+0.03 mJ/m2^{2}, (g) Experimental values with applied field tilted 2∘2^\circ from zz-axis along the xx direction, (h) Ms=Ms,0+0.1M_{s}=M_{s,0}+0.1 MA/m and Ku=Ku,0+0.14K_{u}=K_{u,0}+0.14 MJ/m3^{3}, (i) Ms=Ms,0+0.175M_{s}=M_{s,0}+0.175 MA/m and Ku=Ku,0+0.26K_{u}=K_{u,0}+0.26 MJ/m3^{3}, and (j) Ms=Ms,0+0.1375M_{s}=M_{s,0}+0.1375 MA/m and Ku=Ku,0+0.20K_{u}=K_{u,0}+0.20 MJ/m3^{3}, which represents the best fit. The blue dots represent the experimental data.

dmdt=−∣γ0∣m×Heff+αm×dmdt,(1)\frac{\mathrm{d}\mathbf{m}}{\mathrm{d}t}=-\lvert\gamma_{0}\rvert\mathbf{m}\times\mathbf{H}_{\mathrm{eff}}+\alpha\mathbf{m}\times\frac{\mathrm{d}\mathbf{m}}{\mathrm{d}t}, \tag*{(1)}

where ∥m(r,t)∥=1\lVert\mathbf{m}(\mathbf{r},t)\rVert= 1 is a unit vector representing the orientation of the magnetisation field, γ0=μ0gμB/ℏ\gamma_{0} = \mu_{0}g\mu_{\mathrm{B}}/\hbar is the gyromagnetic constant, and α\alpha is the Gilbert damping constant. The effective field, Heff=−(1/μ0Ms)δU/δm\mathbf{H}_{\mathrm{eff}} = -(1/\mu_{0}M_{\mathrm{s})\delta U/\delta\mathbf{m}}, represents a variational derivative of the total magnetic energy UU with respect to the magnetisation, where UU contains contributions from the Zeeman, nearest-neighbour Heisenberg exchange, interfacial Dzyaloshinskii-Moriya, and dipole-dipole interactions along with uniaxial anisotropy with an easy axis along z^\hat{z}, perpendicular to the film plane. Note that while the lateral cell size of 7.8125 nm used for the simulations presented here is larger than the characteristic exchange length, ℓex=2A/μ0Ms2≃3.65 nm\ell_{\mathrm{ex}} = \sqrt{2A/\mu_{0}M_{\mathrm{s}}^{2}} \simeq3.65\ \mathrm{nm}, we have verified that using smaller discretisation cells do not affect the salient features presented here (see Supplementary Figure 13).

Mesh size dependence of dynamic susceptibility

Supplementary Figure 13. Mesh size dependence of dynamic susceptibility. Simulated imaginary part of the dynamic susceptibility, Im⁡[χ(f)]\operatorname{Im}[\chi(f)], as a function of applied perpendicular field, μ0Hz\mu_{0}H_{z}, for three finite-difference discretization schemes of the 1000×1000×721000 \times1000 \times72 nm simulation box: (a) 128×128×60128 \times128 \times60, (b) 256×256×60256 \times256 \times60, and (c) 512×512×60512 \times512 \times60 finite difference cells. The discretisation scheme and corresponding cell size is indicated on each figure. The micromagnetic parameters used correspond to the experimental values [see Supplementary Figure 12.]

To simulate quasi-static processes such as hysteresis loops, we begin with a uniform magnetic state oriented along −z-z under an applied field of μ0Hz=−500 mT\mu_{0}H_{z} = -500\ \mathrm{mT}. A Langevin-dynamics simulation with T=300 KT = 300\ \mathrm{K} is then performed over 1 ns to mimic experimental conditions in which thermal fluctuations help to sample different metastable states in the energy landscape. The system is then relaxed without the precessional term in Eq. (1) toward an energy minimum. This procedure of running Langevin dynamics, followed by relaxation, is then repeated two more times. After this, the micromagnetic configuration is recorded and assigned as the equilibrium state for the applied field value. This equilibrium state then serves as the initial state for the next value of the applied field, which is increased to μ0Hz=500\mu_0 H_z = 500 mT in increments of 1 mT. The simulated MFM images are computed from the equilibrium state by assuming a sample-to-tip distance of 50 nm.

To simulate the microwave susceptibility of the FeCoB multilayer, we compute the response of the magnetisation to harmonic excitation fields. While it is common practice (and usually more efficient computationally) to calculate the eigenmode spectra from the Fourier transform of the transient response to pulsed fields, such an approach for the present system results in strong artifacts arising from non-resonant drift of the background magnetic state, such as the displacement of the skyrmion lattice or labyrinthine domain structure. Instead, we adopt an approach that more closely resembles the experimental protocol. For each value of the external field HzH_z, we compute the response of the precomputed static configuration, m0(r)\mathbf{m}_0(\mathbf{r}), to sinusoidal in-plane fields with frequency ff, hx=hrfsin⁡(2πft)h_x = h_\mathrm{rf} \sin(2\pi f t), over 20 periods τ=1/f\tau= 1/f, where the spatial average of the resulting component mx(t)m_x(t) is recorded at intervals of 0.1τ0.1\tau. In this procedure, the Gilbert damping parameter is set to α=0.02\alpha= 0.02 and the excitation amplitude to μ0hrf=0.1\mu_0 h_\mathrm{rf} = 0.1 mT (1 mT in Figure 5 and Supplementary Figure 12). We estimate the imaginary part of the susceptibility χ\chi at this frequency, Im⁡[χ(f)]\operatorname{Im}[\chi(f)], by projecting ⟨mx(t)⟩\langle m_x(t)\rangle onto −cos⁡(2πft)-\cos(2\pi f t),

Im⁡[χ(f)]=−120τ∫020τ⟨mx(t)⟩cos⁡(2πft) dt,(2)\operatorname{Im}[\chi(f)] = -\frac{1}{20\tau}\int_0^{20\tau} \langle m_x(t)\rangle\cos(2\pi f t)\,\mathrm{d}t, \tag*{(2)}

which is the quantity shown in Figure 4(a) and Figure 4(b). Im⁡[χ(f)]\operatorname{Im}[\chi(f)] exhibits peaks at resonance when mxm_x is in perfect quadrature with respect to hxh_x. This procedure is repeated as a function of ff ranging from 0.1 GHz to 20 GHz in steps of 0.1 GHz for the map in Figure 4(a) and in steps of 0.02 GHz for the data in Figure 4(b,Figure 4c).

The spatial mode profile at a given mode resonance fnf_n is extracted by driving the system harmonically at fnf_n with hx=hrfsin⁡(2πfnt)h_x = h_\mathrm{rf}\sin(2\pi f_n t) and by recording, cell-by-cell, the components of magnetisation at intervals of 0.1τn0.1\tau_n, as for the calculation of the susceptibility. The mode profiles are characterised by the fluctuation amplitude ⟨δmx(r)⟩\langle\delta m_x(\mathbf{r})\rangle, which is computed in an analogous way to the susceptibility, where we drive the system over 100 periods and then compute, after transients are washed out,

⟨δmx(r)⟩=−12τn∫02τn[mx(r,t)−mx,0(r)]cos⁡(2πfnt) dt,(3)\langle\delta m_x(\mathbf{r})\rangle= -\frac{1}{2\tau_n}\int_0^{2\tau_n} [m_x(\mathbf{r},t)-m_{x,0}(\mathbf{r})]\cos(2\pi f_n t)\,\mathrm{d}t, \tag*{(3)}

over two additional periods. Visually, dark blue regions contribute most to the overall Im⁡[χ(f)]\operatorname{Im}[\chi(f)], while equally dark red and blue regions cancel each other out because they represent fluctuations with opposite sign.

Data availability

Data are available from the corresponding authors upon reasonable request.

Acknowledgements

This work was partially supported by the French National Research Agency (ANR) under grant no. ANR-17-CE24-0025 (TOPSKY) and the Horizon2020 Research Framework Programme of the European Commission under grant nos. 824123 (SKYTOP) and 899646 (k-NET). It is also supported by a public grant overseen by the ANR as part of the “Investissements d’Avenir” program (Labex NanoSaclay, reference: ANR-10-LABX-0035).

Author contributions

N.R., V.C., T.D., J.-V.K and G.d.L. conceived the project. The samples were designed, grown and characterised by T.S., Y.S., F.A., N.R. and V.C. T.S. performed the MFM experiments with the help of A.V. and K.B. H.H. conducted the cavity-FMR measurements. T.S. and I.N. performed initial FMR characterizations. T.D. conducted the VNA-FMR experiments and analyzed the results with T.S. and G.d.L. J.-V.K. performed the micromagnetic simulations and analyzed them with T.S. and G.d.L. T.S., J.-V.K. and G.d.L. wrote the manuscript. All the authors discussed the data and commented on the manuscript.

Competing interests

The authors declare no competing interests.

Additional information

Supplementary information The online version contains supplementary material available at https://doi.org/xxxx.

Correspondence and requests for materials should be addressed to T.S., J.-V.K. or G.d.L.

Supplementary Information — “Resonant dynamics of skyrmion lattices in thin film multilayers: Localised modes and spin wave emission”

Titiksha Srivastava; Yanis Sassi; Fernando Ajejas; Aymeric Vecchiola; Igor Ngouagnia; Hervé Hurdequint; Karim Bouzehouane; Nicolas Reyren; Vincent Cros; Thibaut Devolder; Joo-Von Kim; Grégoire de Loubens

Additional FMR measurements in the saturated state

Angle dependent cavity-FMR

Cavity-FMR measurements are performed at a fixed frequency of 9.725 GHz to probe the FMR of the multilayer sample as a function of the angle θH\theta_H between the applied field and the film plane. Out-of-plane (OP) and in-plane (IP) configurations correspond to θH=0∘\theta_H = 0^\circ and θH=90∘\theta_H = 90^\circ, respectively. The resonant field measured at θH=0∘\theta_H = 0^\circ is higher than at θH=90∘\theta_H = 90^\circ, meaning that the overall anisotropy is in-plane. From the values of the resonant field in these two configurations, one can extract the gyromagnetic ratio γ0/(2π)=28.75\gamma_0/(2\pi) = 28.75 GHz/T and the total uniaxial anisotropy field including demagnetising and PMA contributions μ0(Ms−Hk)=354.7\mu_0(M_s-H_k) = 354.7 mT. Using these values, the full angular variation of the resonance field is accurately reproduced by the theoretical expectation [1], as shown by the continuous line in Supplementary Figure 1(a). The angular dependence of the full width ΔH\Delta H at half maximum of the resonance peak is displayed in Supplementary Figure 1(b). The minimal value of 33.2 mT is observed in the IP configuration, while the linewidth is only slightly larger in the OP configuration, ΔH=35.5\Delta H = 35.5 mT; it is rather low for this type of multilayer film, which evidences its good dynamical quality.

Damping parameter

To separate the intrinsic and extrinsic contributions to the FMR linewidth, broadband-FMR measurements are performed in the IP configuration. At 10 GHz, the extracted linewidth is 32.5 mT, in good agreement with the cavity-FMR results. The frequency dependence of ΔH\Delta H is plotted in Supplementary Figure 1(c) together with its linear fit. The latter yields the frequency independent contribution to the linewidth, found to be about 18 mT, which indicates a fair amount of inhomogeneities in the film. The frequency linear part of the linewidth yields the Gilbert damping parameter of the film, α=0.022±0.003\alpha= 0.022 \pm0.003.

Analysis of the high frequency mode

Internal field in skyrmion lattice phase

The spatial profile of the total internal field (i.e., the sum of the applied, anisotropy, and dipolar fields) can be obtained from micromagnetic simulations. The map obtained at 300 mT is shown for layer 12 in Supplementary Figure 10. It shows that sufficiently far away from the skyrmions, the static internal field is rather homogeneous in the background domains, around 110 to 120 mT. Due to the strong dipolar fields in the vicinity of the oppositely magnetised skyrmion cores, the internal field substantially increases while approaching the skyrmion boundaries, as shown by the closely spaced isocontours. Inside the skyrmion cores it becomes negative, about −200 mT.

Contributions to the eigenfrequency

As shown by Figure 5 of the main text the high frequency mode (HFM) corresponds to a precession of the magnetisation localized inside the skyrmion cores. Its frequency can be calculated as the convolution of its spatial profile with a frequency operator taking into account all the contributions to the magnetic energy (Eq. 8 in ref. [2]): Zeeman, anisotropy, dipolar and exchange energies. Even for homogeneously magnetised non-ellipsoidal bodies, it is difficult to evaluate the magnetic self-interactions (magneto-dipolar and inhomogeneous exchange) contributing to the eigenfrequency. As shown in Figure 3 of the main text, the static configuration in the 20 dipolarly coupled magnetic layers is quite complex in the skyrmion phase. However, to roughly estimate the HFM frequency, one can consider the averaged value of the static internal field inside the skyrmion core where the precession is localized, to which the dynamic magneto-dipolar self-interaction (i.e. the depolarization energy of the mode profile on itself) and the exchange contributions should be added. The averaged value μ0Heff,0≈−200 mT\mu_0 H_{\mathrm{eff},0} \approx-200\ \mathrm{mT} of the internal field in the core translates into a frequency of 5.8 GHz, which is less than the HFM frequency of 15.5 GHz determined by micromagnetic simulations. The exchange contribution to the frequency is given by (γ0AkHFM2)/(πMs)(\gamma_0 A k_{\mathrm{HFM}}^2)/(\pi M_s) where kHFMk_{\mathrm{HFM}} is the effective wavevector of the mode. Assuming an effective wavelength of the order of the skyrmion diameter ≈100 nm\approx100\ \mathrm{nm}, one obtains an exchange contribution of 2.6 GHz. The evaluation of the contribution due to the dynamic magneto-dipolar self-interaction is more difficult, because it requires the knowledge of static and dynamic magnetisation profiles to perform the required integration. However, the missing 7.1 GHz fall in the frequency range of this contribution in submicron samples [2].

Characteristics of the spin waves emitted by the skyrmion cores

To find the characteristics of the spin waves (SWs) emitted by the precession of the skyrmion cores in the surrounding background domains, one should consider that the latter are homogeneously magnetised OP along the applied field and use the dispersion relation of forward-volume waves [3]:

ω(k)=(ωHeff,0+2Aγ0Msk2)(ωHeff,0+2Aγ0Msk2+ωM(1−1−e−ktkt))(4)\omega(k)=\sqrt{\left(\omega_{\mathrm{Heff},0}+\frac{2A\gamma_0}{M_s}k^2\right)\left(\omega_{\mathrm{Heff},0}+\frac{2A\gamma_0}{M_s}k^2+\omega_M\left(1-\frac{1-e^{-kt}}{kt}\right)\right)} \tag*{(4)}

where ωHeff=γ0Heff,0\omega_{\mathrm{Heff}}=\gamma_0H_{\mathrm{eff},0} and ωM=γ0M\omega_M=\gamma_0M. To take into account the multilayer nature of the film, the dynamic dipolar term is evaluated using an effective film medium of total thickness t=20×(tFeCoB+tPt+tAlOx)=76t=20\times(t_{\mathrm{FeCoB}}+t_{\mathrm{Pt}}+t_{\mathrm{AlOx}})=76 nm and magnetisation M=tFeCoB/(tFeCoB+tPt+tAlOx)Ms=0.42M=t_{\mathrm{FeCoB}}/(t_{\mathrm{FeCoB}}+t_{\mathrm{Pt}}+t_{\mathrm{AlOx}})M_s=0.42 MA/m. This dispersion relation is plotted in Supplementary Figure 10 using μ0Heff,0=110\mu_0H_{\mathrm{eff},0}=110 mT, which corresponds to the mean value of the static internal field in the interskyrmion region at the bias field of 300 mT shown in Supplementary Figure 10. The skyrmion core precession frequency at this field is equal to 15.5 GHz, as indicated by the horizontal dashed line that crosses the dispersion curve at k=105k=105 μm−1\mu\mathrm{m}^{-1}, corresponding to a wavelength of λ=59.8\lambda=59.8 nm. This value is in excellent agreement with the one directly determined from the SW radiation pattern of Figure 5(c) in the main text. Moreover, it is also possible to compute the group velocity Vg=∂ω/∂kV_g=\partial\omega/\partial k of the forward-volume wave in the effective film, which is plotted in Supplementary Figure 10. The group velocity of the SWs propagating at 15.5 GHz is found to be Vg=960V_g=960 m/s. Based on Eq. (4), forward volume SWs exhibit almost circular precession in our material, therefore one can use τ=1/(αω)\tau=1/(\alpha\omega) to evaluate their lifetime. At ω/(2π)=15.5\omega/(2\pi)=15.5 GHz, τ=1/(αω)=0.513\tau=1/(\alpha\omega)=0.513 ns, which allows to estimate the attenuation length of this forward-volume SW, Latt=Vgτ=493L_{\mathrm{att}}=V_g\tau=493 nm.

Supplementary Figures

Skyrmion lattice images and nearest neighbour probability distributions

Figure S2. Skyrmion lattice. (a) MFM image of skyrmions in disordered state at -280 mT, and (b) nearest neighbour (NN) probability distribution. (c) Skyrmion lattice at -190 mT, and (d) its nearest neighbour probability distribution, demonstrating its almost quasi periodic hexagonal structure.

VNA-FMR reflection parameters

Figure S6. VNA-FMR reflection parameters. Real parts of the (a) S11S_{11} and (b) S22S_{22} parameters processed using the derivative divide method. A broad signal between 0.5 GHz and 1.5 GHz is observed on the full field range between −330-330 mT and 390 mT, which corresponds to the simulated low frequency modes (LFM).

Supplementary References

  1. Hurdequint, H. FMR studies of ultrathin permalloy layers sandwiched by Al2O3Al_2O_3. J. Magn. Magn. Mater. 242-245, 521–524 (2002).

  1. Naletov, V. V. et al. Identification and selection rules of the spin-wave eigenmodes in a normally magnetized nanopillar. Phys. Rev. B 84, 224423 (2011).

  1. Kalinikos, B. A. & Slavin, A. N. Theory of dipole-exchange spin wave spectrum for ferromagnetic films with mixed exchange boundary conditions. J. Phys. C 19, 7013 (1986).

References

  1. [1]V. V. Kruglyak, S. O. Demokritov, and D. Grundler, “Magnonics,” J. Phys. D Appl. Phys. 43, 264001 (2010).
  2. [2]M. Krawczyk and D. Grundler, “Review and prospects of magnonic crystals and devices with reprogrammable band structure,” J. Condens. Matter Phys. 26, 123202 (2014).pubmed.ncbi.nlm.nih.gov/24599025
  3. [3]A. Barman, G. Gubbiotti, S. Ladak, A. O. Adeyemi, M. Krawczyk, J. Gräfe, C. Adelmann, S. Cotofana, A. Naeemi, V. I. Vasyuchka, et al., “The 2021 magnonics roadmap,” J. Phys.: Condens. Matter 33, 413001 (2021).DOI
  4. [4]György Csaba, Ádám Papp, and Wolfgang Porod, “Perspectives of using spin waves for computing and signal processing,” Phys. Lett. A 381, 1471–1476 (2017).DOI
  5. [5]Ferran Macià, Andrew D Kent, and Frank C Hoppensteadt, “Spin-wave interference patterns created by spin-torque nano-oscillators for memory and computation,” Nanotechnology 22, 095301 (2011).DOI
  6. [6]Ádám Papp, Wolfgang Porod, Árpád I Csurgay, and György Csaba, “Nanoscale spectrum analyzer based on spin-wave interference,” Sci. Rep. 7, 9245 (2017).DOI
  7. [7]Andrii V. Chumak, Alexander A. Serga, and Burkard Hillebrands, “Magnon transistor for all-magnon data processing,” Nat. Commun. 5, 4700 (2014).DOI
  8. [8]Matías Grassi, Moritz Geilen, Damien Louis, Morteza Mohseni, Thomas Brächer, Michel Hehn, Daniel Stoeffler, Matthieu Baillet, Philipp Pirro, and Yves Henry, “Slow-wave-based nanomagnonic diode,” Phys. Rev. Applied 14, 024047 (2020).DOI
  9. [9]Hugo Merbouche, Martin Collet, Michael Evelt, Vladislav E. Demidov, José Luis Prieto, Manuel Munoz, Jamal Ben Youssef, Grégoire de Loubens, Olivier Klein, Stéphane Xavier, et al., “Frequency filtering with a magnonic crystal based on nanometer-thick yttrium iron garnet films,” ACS Appl. Nano Mater. 4, 121–128 (2021).
  10. [10]Florin Ciubotaru, Thibaut Devolder, Mauricio Manfrini, Christoph Adelmann, and IP Radu, “All electrical propagating spin wave spectroscopy with broadband wavevector capability,” Appl. Phys. Lett. 109, 012403 (2016).DOI
  11. [11]Haiming Yu, G. Duerr, R. Huber, M. Bahr, T. Schwarze, F. Brandl, and D. Grundler, “Omnidirectional spin-wave nanograting coupler,” Nat. Commun. 4, 2702 (2013).DOI
  12. [12]Haiming Yu, O. d’Allivy Kelly, V. Cros, R. Bernard, P. Bortolotti, A. Anane, F. Brandl, F. Heimbach, and D. Grundler, “Approaching sub-micron A4 volume wavelengths in nanomagnet-based microwave technology,” Nat. Commun. 7, 11255 (2016).
  13. [13]Jilei Chen, Tao Yu, Chuanpu Liu, Tao Liu, Marco Madami, Ka Shen, Jianyu Zhang, Sa Tu, Md Shah Alam, Ke Xia, et al., “Excitation of unidirectional exchange spin waves by a nanoscale magnetic grating,” Phys. Rev. B 100, 104427 (2019).DOI
  14. [14]H. Fulara, M. Zahedinejad, R. Khymyn, A. A. Awad, S. Muralidhar, M. Dvornik, and J. Åkerman, “Spin-orbit torque-driven propagating spin waves,” Sci. Adv. 5 (2019), 10.1126/sciadv.aax8467.DOI
  15. [15]Haiming Yu, Jiang Xiao, and Helmut Schultheiss, “Magnetic texture based magnonics,” Phys. Rep. 905, 1–59 (2021).DOI
  16. [16]B. E. Argyle, W. Jantz, and J. C. Slonczewski, “Wall oscillations of domain lattices in underdamped garnet films,” J. Appl. Phys. 54, 3370–3386 (1983).DOI
  17. [17]S. A. Montoya, S. Couture, J. J. Chess, J. C. T. Lee, N. Kent, M.-Y. Im, S. D. Kevan, P. Fischer, B. J. McMorran, S. Roy, V. Lomakin, and E. E. Fullerton, “Resonant properties of dipole skyrmions in amorphous Fe/Gd multilayers,” Phys. Rev. B 95, 224405 (2017).DOI
  18. [18]N. Vukadinovic, M. Labrune, J. Ben Youssef, A. Marty, J. C. Toussaint, and H. Le Gall, “Ferromagnetic resonance spectra in a weak stripe domain structure,” Phys. Rev. B 65, 054403 (2001).DOI
  19. [19]U. Ebels, L. Buda, K. Ounadjela, and P. E. Wigen, “Ferromagnetic resonance excitation of two-dimensional wall structures in magnetic stripe domains,” Phys. Rev. B 63, 174437 (2001).DOI
  20. [20]G. Gubbiotti, G. Carlotti, S. Tacchi, M. Madami, T. Ono, T. Koyama, D. Chiba, F. Casoli, and M. G. Pini, “Spin waves in perpendicularly magnetized Co/Ni(11) multilayers in the presence of magnetic domains,” Phys. Rev. B 86, 014401 (2012).
  21. [21]M. Buess, R. Höllinger, T. Haug, K. Perzlmaier, U. Krey, D. Pescia, M. R. Scheinf ein, D. Weiss, and C. H. Back, “Fourier transform imaging of spin vortex eigenmodes,” Phys. Rev. Lett. 93, 077207 (2004).pubmed.ncbi.nlm.nih.gov/15324274
  22. [22]V. Castel, J. Ben Youssef, F. Boust, R. Weil, B. Pigeau, G. de Loubens, V. V. Naletov, O. Klein, and N. Vukadinovic, “Perpendicular ferromagnetic resonance in soft cylindrical elements: Vortex and saturated states,” Phys. Rev. B 85, 184419 (2012).DOI
  23. [23]Felipe Garcia-Sanchez, Pablo Borys, Rémy Soucaille, Jean-Paul Adam, Robert L. Stamps, and Joo-Von Kim, “Narrow magnonic waveguides based on domain walls,” Phys. Rev. Lett. 114, 247206 (2015).
  24. [24]Kai Wagner, A Kakay, K Schultheiss, A Henschke, T Sebastian, and H Schultheiss, “Magnetic domain walls as reconfigurable spin-wave nanochannels,” Nature Nanotech. 11, 432–436 (2016).DOI
  25. [25]Sebastian Wintz, Vasil Tiberkevich, Markus Weigand, Jörg Raabe, Jürgen Lindner, Artur Erbe, Andrei Slavin, and Jürgen Fassbender, “Magnetic vortex cores as tunable spin-wave emitters,” Nature Nanotech. 11, 948–953 (2016).DOI
  26. [26]G. Dieterle, J. Förster, H. Stoll, A. S. Semisalova, S. Finizio, A. Gangwar, M. Weigand, M. Noske, M. Fähnle, I. Bykova, J. Gräfe, et al., “Coherent excitation of heterosymmetric spin waves with ultrashort wavelengths,” Phys. Rev. Lett. 122, 117202 (2019).DOI
  27. [27]Albert Fert, Nicolas Reyren, and Vincent Cros, “Magnetic skyrmions: advances in physics and potential applications,” Nat. Rev. Mater. 2, 17031 (2017).DOI
  28. [28]C. Moreau-Luchaire, C. Moutafis, N. Reyren, J. Sampaio, C.A.F. Vaz, N. Van Horne, K. Bouzehouane, K. Garcia, C. Deranlot, P. Warnicke, et al., “Additive interfacial chiral interaction in multilayers for stabilization of small individual skyrmions at room temperature,” Nature Nanotech. 11, 444–448 (2016).
  29. [29]Olivier Boulle, Jan Vogel, Hongxin Yang, Stefania Pizzini, Dayane de Souza Chaves, Andrea Locatelli, Tevfik Onur Mentes, Alessandro Sala, Liliana D. Buda-Prejbeanu, Olivier Klein, Mohamed Belmeguenai, et al., “Room temperature chiral magnetic skyrmion in ultrathin magnetic nanostructures,” Nature Nanotech. 11, 449–454 (2016).DOI
  30. [30]Titiksha Srivastava, Marine Schott, Roméo Juge, Viola Krizakova, Mohamed Belmeguenai, Yves Roussigne, Anne Bernand-Mantel, Laurent Ranno, Stefania Pizzini, Salim-Mourad Chérif, et al., “Large-voltage tuning of dzyaloshinskii–moriya interactions: A route toward dynamic control of skyrmion chirality,” Nano Lett. 18, 4871–4877 (2018).
  31. [31]Wanjun Jiang, Pramey Upadhyaya, Wei Zhang, Guoqiang Yu, M. Benjamin Jungfleisch, Frank Y. Fradin, John E. Pearson, Yaroslav Tserkovnyak, Kang L. Wang, Olle Heinonen, Suzanne G. E. tel Velt huis, and Axel Hoffmann, “Blowing magnetic skyrmion bubbles,” Science 349, 283–286 (2015).DOI
  32. [32]Seonghoon Woo, Kai Litzius, Benjamin Krüger, Mi-Young Im, Lucas Caretta, Kornel Richter, Maxwell Mann, Andrea Krone, Robert M Reeve, Markus Weigand, et al., “Observation of room-temperature magnetic skyrmions and their current-driven dynamics in ultrathin metallic ferromagnets,” Nature Mater. 15, 501–506 (2016).
  33. [33]F. Garcia-Sanchez, J. Sampaio, N. Reyren, V. Cros, and J.-V. Kim, “A skyrmion-based spin-torque nano-oscillator,” New J. Phys. 18, 075011 (2016).
  34. [34]G. Finocchio, M. Ricci, R. Tomasello, A. Giordano, M. Lanuzza, V. Puliafito, P. Burrascano, B. Azzerboni, and M. Carpentieri, “Skyrmion based microwave detectors and harvesting,” Appl. Phys. Lett. 107, 262401 (2015).DOI
  35. [35]Fusheng Ma, Yan Zhou, H. B. Braun, and W. S. Lew, “Skyrmion-based dynamic magnetic crystal,” Nano Lett. 15, 4029–4036 (2015).DOI
  36. [36]M. Mruczkiewicz, P. Gruszecki, M. Zelent, and M. Krawczyk, “Collective dynamical skyrmion excitations in a magnonic crystal,” Phys. Rev. B 93, 174429 (2016).
  37. [37]Markus Garst, Johannes Waizner, and Dirk Grundler, “Collective spin excitations of helices and magnetic skyrmions: review and perspectives of magnonics in non-centrosymmetric magnets,” J. Phys. D Appl. Phys. 50, 293002 (2017).DOI
  38. [38]Xi-guang Wang, Yao-Zhuang Nie, Qing-lin Xia, and Guang-hua Guo, “Dynamically reconfigurable magnetic crystal composed of artificial magnetic skyrmion lattice,” J. Appl. Phys. 128, 063901 (2020).DOI
  39. [39]Christoph Schütte and Markus Garst, “Magnon-skyrmion scattering in chiral magnets,” Phys. Rev. B 90, 094423 (2014).DOI
  40. [40]Joo-Von Kim, Felipe Garcia-Sanchez, Joao Sampaio, Constance Moreau-Luchaire, Vincent Cros, and Albert Fert, “Breathing modes of confined skyrmions in ultrathin magnetic dots,” Phys. Rev. B 90, 064410 (2014).DOI
  41. [41]Vanessa Li Zhang, Chen Guang Hou, Kai Di, Hock Siah Lim, Ser Choon Ng, Shawn David Pollard, Hyunsoo Yang, and Meng Hau Kuok, “Eigenmodes of néel skyrmions in ultrathin magnetic films,” AIP Adv. 7, 055212 (2017).DOI
  42. [42]M. Mruczkiewicz, M. Krawczyk, and K. Y. Guslienko, “Spin excitation spectrum in a magnetic nanodot with continuous transitions between the vortex, bloch-type skyrmion, and néel-type skyrmion states,” Phys. Rev. B 95, 094414 (2017).DOI
  43. [43]Volodymyr P. Kravchuk, Denis D. Sheka, Ulrich K. Rößler, Jeroen van den Brink, and Yuri Gaididei, “Spin eigenmodes of magnetic skyrmions and the problem of the effective skyrmion mass,” Phys. Rev. B 97, 064403 (2018).DOI
  44. [44]Y. Onose, Y. Okamura, S. Seki, S. Ishiwata, and Y. Tokura, “Observation of magnetic excitations of skyrmion crystal in a helimagnetic insulator Cu₂OSeO₃,” Phys. Rev. Lett. 109, 037603 (2012).pubmed.ncbi.nlm.nih.gov/22861898
  45. [45]T. Schwarze, J. Waizner, M. Garst, A. Bauer, I. Stasinopoulos, H. Berger, C. Pfleiderer, and D. Grundler, “Universal helimagnon and skyrmion excitations in metallic, semiconducting and insulating chiral magnets,” Nature Mater. 14, 478–483 (2015).DOI
  46. [46]Aisha Aqeel, Jan Sahliger, Takuya Taniguchi, Stefan Mä ndl, Denis Mettus, Helmuth Berger, Andreas Bauer, Markus Garst, Christian Pfleiderer, and Christian H. Back, “Microwave spectroscopy of the low-temperature skyrmion state in Cu₂OSeO₃,” Phys. Rev. Lett. 126, 017202 (2021).DOI
  47. [47]Bhartendu Satywali, Volodymyr P. Kravchuk, Liqing Pan, M. Raju, Shikun He, Fusheng Ma, A. P. Petrovic, Markus Garst, and Christos Panagopoulos, “Microwave resonances of magnetic skyrmions in thin film multilayers,” Nat. Commun. 12, 1909 (2021).DOI
  48. [48]Luis Flacke, Valentin Ahrens, Simon Mendisch, Lukas Körber, Tobias Böttcher, Elisabeth Meidinger, Misbah Yaqoob, Manuel Müller, Lukas Liensberger, Attila Kákay, Markus Becherer, Philipp Pirro, Matthias Althammer, Stephan Geprägs, Hans Huebl, Rudolf Gross, and Mathias Weiler, “Robust formation of nanoscale magnetic skyrmions in easy-plane anisotropy thin film multilayers with low damping,” Phys. Rev. B 104, L100417 (2021).DOI
  49. [49]William Legrand, Jean-Yves Chauleau, Davide Maccariello, Nicolas Reyren, Sophie Collin, Karim Bouzehouane, Nicolas Jaouen, Vincent Cros, and Albert Fert, “Hybrid chiral domain walls and skyrmions in magnetic multilayers,” Sci. Adv. 4, eaat0415 (2018).DOI
  50. [50]Hongxin Yang, Olivier Boulle, Vincent Cros, Albert Fert, and Mairbek Chshiev, “Controlling dzyaloshinskii-moriya interaction via chirality dependent atomic-layer stacking, insulator capping and electric field,” Sci. Rep. 8, 12356 (2018).DOI
  51. [51]Nam-Hui Kim, Jaehun Cho, Jinyong Jung, Dong-Soo Han, Yuxiang Yin, June-Seo Kim, Henk J. M. Swagten, Kuyjooon Lee, Myung-Hwa Jung, and Chun-Yeol You, “Role of top and bottom interfaces of a pt/co/alox system in dzyaloshinskii-moriya interaction, interface perpendicular magnetic anisotropy, and magneto-optical Kerr effect,” AIP Adv. 7, 035213 (2017).DOI
  52. [52]S. Tacchi, R. E. Troncoso, M. Ahlberg, G. Gubbiotti, M. Madami, J. Åkerman, and P. Landeros, “Interfacial dzyaloshinskii-moriya interaction in Pt/CoFeB films: Effect of the heavy-metal thickness,” Phys. Rev. Lett. 118, 147201 (2017).DOI
  53. [53]William Legrand, Yanis Sassi, Fernando Ajejas, Sophie Collin, Laura Bocher, Hongying Jia, Markus Hoffmann, Bernd Zimmermann, Stefan Blügel, Nicolas Reyren, Vincent Cros, and André Thiaville, “Spatial extent of the dzyaloshinskii-moriya interaction at metallic interfaces,” Phys. Rev. Materials 6, 024408 (2022).
  54. [54]M. Melbeguenaei, M. S. Gabor, F. Zighem, N. Challab, T. Petrisor, R. B. Mos, and C. Tiusan, “Ferromagnetic-resonance-induced spin pumping in Co₂₀Fe₆₀B₂₀/Pt systems: damping investigation,” J. Phys. D Appl. Phys. 51, 045002 (2018).
  55. [55]Tobias Böttcher, Kyujooon Lee, Frank Heussner, Samridh Jaiswal, Gerhard Jakob, Mathias Kläui, Burkard Hillebrands, Thomas Brächer, and Philipp Pirro, “Heisenberg exchange and dzyaloshinskii-moriya interaction in ultrathin Pt(W)/CoFeB single and multilayers,” IEEE Trans. Magn. 57, 1–7 (2021).DOI
  56. [56]Henryk Puszarski, “Theory of interface magnons in magnetic multilayer films,” Surf. Sci. Rep. 20, 45–110 (1994).
  57. [57]Arne Vansteenkiste, Jonathan Leliaert, Mykola Dvornik, Mathias Helsen, Felipe Garcia-Sanchez, and Bartel Van Waeyenberge, “The design and verification of MuMax3,” AIP Adv. 4, 107133 (2014).DOI
  58. [58]Jilei Chen, Junfeng Hu, and Haiming Yu, “Chiral emission of exchange spin waves by magnetic skyrmions,” ACS Nano 15, 4372–4379 (2021).DOI
  59. [59]M. Sushruth, M. Grassi, K. Ait-Oukaci, D. Stoeffler, Y. Henry, D. Lacour, M. Hehn, U. Bhaskar, M. Bailleul, T. Devolder, and J.-P. Adam, “Electrical spectroscopy of forward volume spin waves in perpendicularly magnetized materials,” Phys. Rev. Research 2, 043200 (2020).
  60. [60]S. Sani, J. Persson, S.M. Mohseni, Ye Pogorelov, P.K. Muduli, A. Eklund, G. Malm, M. Käll, A. Dmitriev, and J. Åkerman, “Mutually synchronized bottom-up multi-nanocontact spin-torque oscillators,” Nat. Commun. 4, 2731 (2013).DOI
  61. [61]Sho Watanabe, Vinayak S. Bhat, Korbinian Baumgaertl, and Dirk Grundler, “Direct observation of worm-like nanochannels and emergent magnon motifs in artificial ferromagnetic quasicrystals,” Adv. Funct. Mater. 30, 2001388 (2020).
  62. [62]Sebastián A. Díaz, Tomoki Hirosawa, Jelena Klinovaja, and Daniel Loss, “Chiral magnonic edge states in ferromagnetic skyrmion crystals controlled by magnetic fields,” Phys. Rev. Research 2, 013231 (2020).DOI
  63. [63]Hannes Maier-Flaig, Sebastian T. B. Goennenwein, Ryo Ohshima, Masashi Shiraishi, Rudolf Gross, Hans Huebl, and Mathias Weiler, “Note: Derivative divide, a method for the analysis of broadband ferromagnetic resonance in the frequency domain,” Rev. Sci. Instrum. 89, 076101 (2018).
  64. [64]Y. Feng, P. Mirzadeh Vaghefi, S. Vranjkovic, M. Penedo, P. Kappernberger, J. Schwenk, X. Zhao, A.-O. Mandru, and H.J. Hug, “Magnetic force microscopy contrast formation and field sensitivity,” J. Magn. Magn. Mater. 551, 169073 (2022).DOI

Paper details

vlnc:W_ugefcmz4
Version
v1 · latest
Published
Fresh — added to the Hub within the last 30 days
Added
License
CC BY 4.0
Usage

views · 0

downloads · 0

A view counts once per browser per day, a download each time the PDF is requested.

  • Physics and Astronomy

Not recorded for this paper

View statement
Looking for related papers…
Contents