Dopant-vacancy complexes as single-photon-emitter candidates in monolayer silicon carbide: radiative and nonradiative decay

Abstract

Solid-state color centers have emerged as promising single-photon sources (SPSs). In particular, color centers in two-dimensional (2D) materials combine high photon brightness with scalable fabrication and ease of integration, offering a versatile platform for quantum information technologies. Realizing high-efficiency SPSs, however, requires strong radiative emission and negligible nonradiative decay. Using first-principles calculations, we assess radiative and nonradiative decay in dopant-vacancy complexes XSiVC (X = N, O, P, and S) in monolayer silicon carbide. All four defects exhibit stable neutral charge states and inter-defect optical transitions. Among them, PSiVC emerges as the leading single-photon-emitter candidate, combining rapid radiative decay with negligible nonradiative decay and a near-unity quantum yield within the modeled channels. By contrast, multiphonon decay limits the quantum yield of NSiVC despite its high Debye-Waller factor. Hyperfine tensors provide characteristic signatures for identifying the spin-active centers. Beyond identifying promising candidates, these results establish a joint radiative-nonradiative screening strategy and provide theoretical guidance for the rational design of color centers as solid-state SPSs.

Introduction

Solid-state color centers have emerged as promising single-photon emitters (SPEs) for quantum-information technologies [1, 2], including quantum key distribution [3], quantum repeaters [4], quantum metrology [5], and quantum sensing [6, 7, 8, 9]. These defects create atomlike localized states within the host band gap, enabling well-isolated optical transitions and, in many cases, optically addressable spin states, while preserving the robustness and scalability of solid-state hosts.

Diamond color centers established solid-state SPEs [10, 11, 12, 13]. However, the NV−^{-} center, despite its excellent spin properties, has a Debye–Waller (DW) factor of only ~3%, with most emission occurring in the phonon sideband. Group-IV centers such as SiV−^{-} and SnV−^{-} offer much higher DW factors (up to 0.7–0.9 for SiV−^{-}), yet simultaneously achieving high single-photon efficiency and scalable, cavity-free operation in diamond remains challenging [14, 15, 16, 17, 18, 19, 20].

Silicon carbide (SiC) offers a technologically mature alternative to diamond [4, 13, 21]. Ultrabright, photostable SPSs operating at room temperature have been demonstrated [22, 23, 24], and subsequent advances are reviewed in Ref. [25]. However, precise defect positioning and efficient photon extraction remain challenging in bulk crystals. Their high refractive indices limit photon extraction through total internal reflection, while deeply embedded defects are difficult to access and couple to photonic structures. In contrast, 2D hosts place emitters at or near their surfaces, facilitating photon extraction, defect engineering, and heterogeneous integration with photonic and electrical devices [26, 27, 28]. Defect-related SPEs in 2D materials have been reported in hexagonal boron nitride [8, 29, 30, 31, 32, 33, 34, 35], transition-metal dichalcogenides [36, 37, 38, 39, 40, 41, 42], and other 2D systems [43, 44]. Among these hosts, monolayer SiC is particularly attractive because it combines a wide band gap with nuclear-spin-free elements. Experiments have demonstrated environmentally stable 2D-SiC nanoflakes with visible emission [45]. Nearly planar, millimeter-scale monocrystalline SiC monolayers have also been reported and remain stable in vacuum up to approximately 1200 °C [46]. These results establish the 2D-SiC monolayer as a processable, thermally robust host platform suitable for defect-based quantum emitters. First-principles studies have proposed several native defects and impurity-related centers in monolayer SiC as candidate SPEs. [47, 48, 49, 50]. However, the competition between radiative emission and nonradiative decay in these complexes requires systematic assessment to reliably evaluate their potential as high-efficiency SPEs [51, 52].

Here, we use first-principles calculations with the HSE06 hybrid functional to investigate dopant–vacancy complexes XSi_{\mathrm{Si}}VC_{\mathrm{C}} (X = N, O, P, and S) in monolayer SiC. The XC_{\mathrm{C}}VSi_{\mathrm{Si}} color centers have been previously investigated, which have the reverse defect configuration [50]. The assessment covers charge-state stability, localized optical transitions, electron–phonon coupling, and competing radiative and nonradiative decay pathways. Calculated hyperfine tensors and spin densities to characterize the spin-active centers and provide fingerprints for their experimental detection. Among these defects, neutral PSi_{\mathrm{Si}}VC_{\mathrm{C}} emerges as the most promising SPE candidate, combining fast radiative decay with negligible nonradiative loss.

Computational details

DFT computational parameters

Spin-polarized density functional theory (DFT) calculations were performed using the Vienna Ab initio Simulation Package (VASP, version 5.4) [53, 54]. Electron–ion interactions were treated using the projector-augmented-wave (PAW) method [55, 56], with a plane-wave energy cutoff of 520 eV. Structural relaxations were performed within the Perdew–Burke–Ernzerhof (PBE) generalized-gradient approximation (GGA) [57]. Electronic properties were calculated using the Heyd–Scuseria–Ernzerhof (HSE06) hybrid functional, with an exact exchange fraction of 25% and a screening parameter of 0.2 Å−1^{-1} [58, 59].

Each XSi_{\mathrm{Si}}VC_{\mathrm{C}} defect (X = N, O, P, or S) was modeled in an 8 × 8 × 1 supercell of pristine 2D-SiC containing 128 atoms. The supercell was based on our previously reported model [49, 50].

Each defect was created by replacing one Si atom with a dopant and removing a neighboring C atom. A vacuum spacing of approximately 20 Å was used to minimize interactions between periodic images. The Brillouin zone was sampled using the Monkhorst–Pack scheme [60], with only the Γ\Gamma point used for the supercell calculations. Gaussian smearing with a width of 0.05 eV was used. Atomic coordinates were optimized using the conjugate-gradient algorithm while keeping the lattice vectors fixed. The energy and force convergence criteria were set to 10−410^{-4} eV and 0.02 eV Å−1^{-1}, respectively. For electron–phonon coupling calculations, these criteria were tightened to 10−510^{-5} eV and 0.001 eV Å−1^{-1}. Phonon spectra were calculated using PHONOPY [61]. Excited-state geometries were optimized using the constrained-occupation Δ\DeltaSCF (self-consistent-field) method [62].

Theoretical formalism

The formation energy is defined as

Efq=Etotq−Etotper+Ecorrq−∑iniμi+q(EF+EVBM)(1)E_f^q = E_{\mathrm{tot}}^q - E_{\mathrm{tot}}^{\mathrm{per}} + E_{\mathrm{corr}}^q - \sum_i n_i\mu_i + q(E_F + E_{\mathrm{VBM}}) \tag*{(1)}

where EtotqE_{\mathrm{tot}}^q and EtotperE_{\mathrm{tot}}^{\mathrm{per}} are the total energies of the defective supercell in charge state qq and the neutral pristine supercell, respectively. EcorrqE_{\mathrm{corr}}^q is the finite-size electrostatic correction for the charged 2D supercell. It was evaluated using the Freysoldt–Neugebauer scheme [63] implemented in sxdefectalign2d [64]. Here, nin_i is the number of atoms of species ii added (positive) to or removed (negative) from the supercell, and μi\mu_i is the corresponding chemical potential. For the present complexes, ∑iniμi=μX−μSi−μC=μX−(μSi+μC)=μX−μSiC\sum_i n_i\mu_i = \mu_X - \mu_{\mathrm{Si}} - \mu_{\mathrm{C}} = \mu_X - (\mu_{\mathrm{Si}} + \mu_{\mathrm{C}}) = \mu_X - \mu_{\mathrm{SiC}}, where μSiC\mu_{\mathrm{SiC}} is the total energy of the 2D-SiC primitive cell. μX\mu_X is the chemical potential of element X (X = N, O, P, or S) in the reference phase specified in Table S1. The calculated chemical potentials are also reported in Table S1. EVBME_{\mathrm{VBM}} denotes the valence-band maximum (VBM) of the pristine supercell. The Fermi level, EFE_F, is referenced to the VBM and varied across the band gap.

The binding energy is defined as

Eb(XSiVC)=Efmin⁡(XSi)+Efmin⁡(VC)−Efmin⁡(XSiVC)(2)E_b(\mathrm{X}_{\mathrm{Si}}\mathrm{V}_{\mathrm{C}})=E_f^{\min}(\mathrm{X}_{\mathrm{Si}})+E_f^{\min}(\mathrm{V}_{\mathrm{C}})-E_f^{\min}(\mathrm{X}_{\mathrm{Si}}\mathrm{V}_{\mathrm{C}}) \tag*{(2)}

where Efmin⁡(XSi)E_f^{\min}(\mathrm{X}_{\mathrm{Si}}) and Efmin⁡(VC)E_f^{\min}(\mathrm{V}_{\mathrm{C}}) are the minimum formation energies of the isolated XSi\mathrm{X}_{\mathrm{Si}} and VC\mathrm{V}_{\mathrm{C}} defects, respectively. The quantity Efmin⁡(XSiVC)E_f^{\min}(\mathrm{X}_{\mathrm{Si}}\mathrm{V}_{\mathrm{C}}) is the corresponding minimum formation energy of the defect complex.

The transition dipole moment (TDM) is defined as

μ=iℏ(Eb−Ea)m⟨ψa∣p^∣ψb⟩(3)\mu=\frac{i\hbar}{(E_b-E_a)m}\langle\psi_a|\hat{p}|\psi_b\rangle \tag*{(3)}

where ψa\psi_a and ψb\psi_b are the initial- and final-state wave functions with energy eigenvalues EaE_a and EbE_b, respectively, mm is the electron mass, ℏ\hbar is the reduced Planck constant, and p^\hat{p} is the momentum operator. The TDMs were calculated at the HSE06 level and processed using the VASP toolkit (vaspkit) [65].

The total Huang–Rhys (HR) factor (SS) is given by

S=∑k=1MSk,Sk=ωkΔQk22ℏ(4)S=\sum_{k=1}^{M}S_k,\quad S_k=\frac{\omega_k\Delta Q_k^2}{2\hbar} \tag*{(4)}

where MM is the number of vibrational modes and kk is the mode index. The quantities ωk\omega_k and QkQ_k are the frequency of the kthk^{\mathrm{th}} vibrational mode and the mass-weighted displacement projected onto this mode, respectively.

The photoluminescence (PL) spectrum is given by

Iem(ℏω)=ω3⋅12π∫−∞+∞G(t)eiωte−γ∣t∣ dt(5)I_{\mathrm{em}}(\hbar\omega)=\omega^3\cdot\frac{1}{2\pi}\int_{-\infty}^{+\infty}G(t)e^{i\omega t}e^{-\gamma|t|}\,dt \tag*{(5)}

where γ\gamma is the zero-phonon-line (ZPL) linewidth and G(t)G(t) is the generating function. The HR factors and PL spectra were calculated using PyPhotonics [66].

The radiative lifetime is given by [67]:

1τrad=nEZPL3∣μ∣23πε0c3ℏ4(6)\frac{1}{\tau_{\mathrm{rad}}} = \frac{n E_{\mathrm{ZPL}}^{3} \lvert\mu\rvert^{2}}{3\pi\varepsilon_{0} c^{3} \hbar^{4}} \tag*{(6)}

where τrad\tau_{\mathrm{rad}} is the radiative lifetime, and nn is the refractive index of 2D-SiC, taken as approximately 2.65 was used [48]. The quantities EZPLE_{\mathrm{ZPL}} and μ\mu denote the ZPL energy and corresponding TDM, respectively. ε0\varepsilon_{0}, cc and ℏ\hbar are the vacuum permittivity, the speed of light, and the reduced Planck constant, respectively.

Nonradiative transition rates and lifetimes were calculated using Nonrad [68] within a one-dimensional configuration-coordinate model. This approach describes multiphonon transitions between electronic states using Fermi's golden rule in the static-coupling approximation. The nonradiative transition coefficient is given by

C=f2πℏgV∣Wif∣2∑mwm∑n∣⟨χim∣Q^−Q0∣χfn⟩∣2×δ(Δε+mℏΩi−nℏΩf)(7)C = f \frac{2\pi}{\hbar} gV \lvert W_{if} \rvert^{2} \sum_{m} w_{m} \sum_{n} \left\lvert\langle\chi_{im} \lvert\hat{Q} - Q_{0} \rvert\chi_{fn} \rangle\right\rvert^{2} \times\delta(\Delta\varepsilon+ m\hbar\Omega_{i} - n\hbar\Omega_{f}) \tag*{(7)}

where ff is a scaling factor, gg is the configurational degeneracy, and VV is the supercell volume. The configurational degeneracy was set to 1 for all transitions considered here. WifW_{if} is the electron–phonon coupling matrix element, and wmw_{m} is the thermal occupation of the mm-th vibrational level of the initial state. The initial and final electronic states correspond to the localized excited state and ground state, respectively. These states have vibrational wave functions χim\chi_{im} and χfn\chi_{fn}, respectively, and an energy difference of Δε\Delta\varepsilon. Their harmonic phonon frequencies are Ωi\Omega_{i} and Ωf\Omega_{f}, respectively. Here, QQ is the mass-weighted configuration coordinate, and Q0Q_{0} is the reference atomic configuration. The mass-weighted displacement between the relaxed initial- and final-state structures is denoted by ΔQ\Delta Q. The values of ΔQ\Delta Q and Δε\Delta\varepsilon used in the calculations are listed in Table S2. For these localized-state transitions, VV and ff were set to unity, so Eq. (7) yields a transition rate in s−1\mathrm{s}^{-1}.

The hyperfine tensor (Aij)(A_{ij}) provides a microscopic spin signature and comprises isotropic Fermi-contact and anisotropic dipolar contributions:

Aij=23μ0γeγIδij⟨Sz⟩∫δT(r⃗)ρs(r⃗+R⃗I) dr⃗+μ04πγeγI⟨Sz⟩∫ρs(r⃗+R⃗I)r33rirj−δijr2r2 dr⃗(8)A_{ij} = \frac{2}{3}\frac{\mu_0\gamma_e\gamma_I\delta_{ij}}{\langle S_z\rangle}\int\delta_T(\vec{r})\rho_s(\vec{r}+\vec{R}_I)\,\mathrm{d}\vec{r}+\frac{\mu_0}{4\pi}\frac{\gamma_e\gamma_I}{\langle S_z\rangle}\int\frac{\rho_s(\vec{r}+\vec{R}_I)}{r^3}\frac{3r_i r_j-\delta_{ij}r^2}{r^2}\,\mathrm{d}\vec{r} \tag*{(8)}

where μ0\mu_0 is the vacuum permeability, and γe\gamma_e and γI\gamma_I are the electron and nuclear gyromagnetic ratios, respectively. Here, ⟨Sz⟩\langle S_z\rangle is the expectation value of the z-component of the total electron spin, ρs\rho_s is the spin density, and δT(r⃗)\delta_T(\vec{r}) is a broadening function. The nuclear position is R⃗I\vec{R}_I, and rir_i denotes the ithi^{\mathrm{th}} Cartesian component of r⃗\vec{r}, with r=∣r⃗∣r=|\vec{r}|.

Results and Discussion

Structural reconstruction and charge-state stability

Fig. S1 shows the optimized XSiVC\mathrm{X}_{\mathrm{Si}}\mathrm{V}_{\mathrm{C}} structures (X=N\mathrm{X}=\mathrm{N}, O, P, and S) in monolayer SiC. Figure 1(a) highlights the local reconstruction, with the arrow indicating an enlarged view of the relaxed defect. Two Si atoms adjacent to the C vacancy formed a Si–Si bond, producing a five-membered ring while preserving the C2vC_{2v} symmetry of the defect complex. This reconstruction is common to all four complexes and defines the local environment for the optical transitions discussed below.

Defect configurations, electronic densities of states, and formation energies

Figure 1. Defect configurations (a), electronic densities of states (b), and formation energies (c) of XSiVC\mathrm{X}_{\mathrm{Si}}\mathrm{V}_{\mathrm{C}} (X = N, O, P, and S). Brown, blue, and yellow spheres represent C, Si, and substitutional dopant atoms, respectively. In panel (c), pale blue and green shaded regions indicate the valence band (VB) and conduction band (CB), respectively. Electronic structures and formation energies were calculated using HSE06.

The HSE06 density of states (DOS) in Figure 1(b) shows localized states within the host band gap. OSiVC\mathrm{O}_{\mathrm{Si}}\mathrm{V}_{\mathrm{C}} and SSiVC\mathrm{S}_{\mathrm{Si}}\mathrm{V}_{\mathrm{C}} have closed-shell (S=0S=0) ground states, whereas NSiVC\mathrm{N}_{\mathrm{Si}}\mathrm{V}_{\mathrm{C}} and PSiVC\mathrm{P}_{\mathrm{Si}}\mathrm{V}_{\mathrm{C}} have doublet ground states (S=1/2S=1/2). The spin-resolved defect levels and associated optical transitions are examined in § 3 B.

Figure 1(c) compares the formation energies of the +1+1, 0, and −1-1 charge states, and Table 1 lists the charge-transition levels. NSiVC\mathrm{N}_{\mathrm{Si}}\mathrm{V}_{\mathrm{C}} changed from positive to neutral at a (+∣0)(+|0) level of 1.190 eV. OSiVC\mathrm{O}_{\mathrm{Si}}\mathrm{V}_{\mathrm{C}} supported three charge states, with (+∣0)(+|0) and (0∣−)(0|-) transition levels at 0.675 and 2.799 eV, respectively. PSiVC\mathrm{P}_{\mathrm{Si}}\mathrm{V}_{\mathrm{C}} remained neutral throughout the pristine-supercell band gap, giving it the broadest neutral-state stability range among the four defects. For SSiVC\mathrm{S}_{\mathrm{Si}}\mathrm{V}_{\mathrm{C}}, the (+∣0)(+|0) and (0∣−)(0|-) levels were 0.709 and 3.323 eV, respectively. Its negative charge state was stable only in the 0.203 eV interval below the conduction-band minimum (CBM), located at 3.526 eV. All four defects possess thermodynamically stable neutral charge states, which are the focus of the following analysis. The positive binding energies in Fig. S2 further confirm that XSiVC\mathrm{X}_{\mathrm{Si}}\mathrm{V}_{\mathrm{C}} complex formation is thermodynamically favorable relative to isolated XSi\mathrm{X}_{\mathrm{Si}} and VC\mathrm{V}_{\mathrm{C}} defects.

Defectsε(+∣0)\varepsilon(+|0)ε(0∣−)\varepsilon(0|-)
NSi_{\mathrm{Si}}}VC_{\mathrm{C}}}1.1906.658
OSi_{\mathrm{Si}}}VC_{\mathrm{C}}}0.6752.799
PSi_{\mathrm{Si}}}VC_{\mathrm{C}}}-0.2094.425
SSi_{\mathrm{Si}}}VC_{\mathrm{C}}}0.7093.323

Table 1. HSE06 charge-transition levels (ε\varepsilon) of XSi_{\mathrm{Si}}}VC_{\mathrm{C}}} (X = N, O, P, and S) relative to the pristine-supercell VBM, in eV. The pristine-supercell band gap is 3.526 eV.

Localized defect levels and optical transitions

Figure 2 shows the in-gap defect levels and corresponding Kohn–Sham wave functions of neutral XSi_{\mathrm{Si}}}VC_{\mathrm{C}}} defects (X = N, O, P, and S). The levels are labeled by the irreducible representations of the defect point group. The occupied 1b2_2 and lowest unoccupied 2b2_2 states in the spin-up channel supported spin-conserving 1b2_2 → 2b2_2 transitions in NSi_{\mathrm{Si}}}VC_{\mathrm{C}}} and PSi_{\mathrm{Si}}}VC_{\mathrm{C}}}. The occupied 1b2_2 and lowest unoccupied 2b2_2 states in both spin channels supported spin-conserving 1b2_2 → 2b2_2 transitions in OSi_{\mathrm{Si}}}VC_{\mathrm{C}}} and SSi_{\mathrm{Si}}}VC_{\mathrm{C}}}. The wave functions were concentrated around the vacancy, dopant, and neighboring Si–C framework, confirming strongly localized optical excitation.

In-gap defect levels and Kohn–Sham wave functions of neutral NSiVC, OSiVC, PSiVC, and SSiVC

Figure 2. In-gap defect levels and Kohn–Sham wave functions of neutral NSiVCN_{\mathrm{Si}}V_{\mathrm{C}} (a), OSiVCO_{\mathrm{Si}}V_{\mathrm{C}} (b), PSiVCP_{\mathrm{Si}}V_{\mathrm{C}} (c), and SSiVCS_{\mathrm{Si}}V_{\mathrm{C}} (d), calculated using HSE06. Red arrows denote electron spins, and green arrows denote optical transitions. The defect levels are labeled by their orbital irreducible representations. Pale blue and green shaded regions indicate the VB and CB, respectively. Light-blue and yellow lobes represent negative and positive wave-function isosurfaces, respectively, with an absolute isosurface value of 10−910^{-9} A˚−3\mathring{\mathrm{A}}^{-3}.

Table 2 reports the separations of the lowest unoccupied and occupied transition levels from the CBM (ΔEC\Delta E_{\mathrm{C}}) and VBM (ΔEV\Delta E_{\mathrm{V}}), respectively. It also lists their energy difference (ΔE\Delta E) and the calculated band gap for each defect. The occupied levels lay 1.095–1.593 eV above the VBM, whereas the lowest unoccupied levels lay 0.625–1.179 eV below the CBM. Their separation from the band edges favors localized excitation. The ΔE\Delta E values ranged from 0.859 eV for NSi_{\mathrm{Si}}}VC_{\mathrm{C}}} to 1.489 eV for PSi_{\mathrm{Si}}}VC_{\mathrm{C}}}. These single-particle energy differences characterize the electronic transitions, whereas emission performance also depends on the relaxed ZPL energies and competing decay rates.

Table 2. HSE06 energy separations of the unoccupied transition level from the CBM (ΔEC\Delta E_{\mathrm{C}}) and of the occupied transition level from the VBM (ΔEV\Delta E_{\mathrm{V}}), and the energy difference between these levels (ΔE\Delta E). All energies are in eV.

DefectΔEC\Delta E_CΔEV\Delta E_VΔE\Delta E
NSiVCN_{\mathrm{Si}}V_{\mathrm{C}}0.9611.5930.859
OSiVCO_{\mathrm{Si}}V_{\mathrm{C}}1.1791.0951.154
PSiVCP_{\mathrm{Si}}V_{\mathrm{C}}0.6251.3171.489
SSiVCS_{\mathrm{Si}}V_{\mathrm{C}}0.9461.1381.420

Table 3.

Magneto-optical properties and spin signatures

An ideal SPE combines high photon purity, indistinguishability, brightness, and stability with a suitable emission wavelength and ease of photonic integration [26]. Here, we assess ZPL energies, TDMs, radiative lifetimes, electron–phonon coupling, and competing relaxation pathways. A high transition energy and large TDM favor rapid radiative decay, whereas the observable photon rate also depends on nonradiative loss and photon extraction. The DW factor quantifies the fraction of emitted light in the ZPL and is distinct from the total luminescence quantum yield.

Table 3 summarizes the optical parameters of the four neutral XSiVCX_{\mathrm{Si}}V_{\mathrm{C}} centers. Their 1b2↑→2b2↑1b_{2}^{\uparrow} \to2b_{2}^{\uparrow} transitions were optically active because of the large wave-function overlap, with TDMs of 5.4–9.2 D and near-infrared ZPL energies of 0.62–1.15 eV. PSiVCP_{\mathrm{Si}}V_{\mathrm{C}} combined the largest TDM (9.2 D) with the highest ZPL energy (1.15 eV), yielding the shortest radiative lifetime (18.2 ns). SSiVCS_{\mathrm{Si}}V_{\mathrm{C}} had the second-shortest radiative lifetime (33.5 ns). Although NSiVCN_{\mathrm{Si}}V_{\mathrm{C}} had a similarly large TDM (9.0 D), its lower ZPL energy (0.62 eV) yielded a radiative lifetime of 120.4 ns. OSiVCO_{\mathrm{Si}}V_{\mathrm{C}} had the smallest TDM and the longest radiative lifetime. These results show that transition energy and dipole strength must be considered together when assessing radiative emission.

Electron–phonon coupling redistributes emission between the ZPL and phonon sideband (PSB), as illustrated by the PL spectra in Figure 3. NSiVCN_{\mathrm{Si}}V_{\mathrm{C}}, PSiVCP_{\mathrm{Si}}V_{\mathrm{C}}, SSiVCS_{\mathrm{Si}}V_{\mathrm{C}}, and OSiVCO_{\mathrm{Si}}V_{\mathrm{C}} had HR factors of 0.65, 1.33, 2.01, and 2.53, respectively, corresponding to DW factors of 52%, 26%, 13%, and 8%. NSiVCN_{\mathrm{Si}}V_{\mathrm{C}} exhibited the largest ZPL fraction and the weakest phonon sidebands, whereas the other defects showed progressively stronger phonon-assisted emission. Its DW factor exceeds earlier predictions for other defects in monolayer SiC [47, 48, 49, 50]. PSiVCP_{\mathrm{Si}}V_{\mathrm{C}} and SSiVCS_{\mathrm{Si}}V_{\mathrm{C}} also exhibited higher ZPL fractions and shorter radiative lifetimes than OSiVCO_{\mathrm{Si}}V_{\mathrm{C}}. We therefore excluded OSiVCO_{\mathrm{Si}}V_{\mathrm{C}} from the subsequent relaxation analysis because it had the longest radiative lifetime (185.3 ns) and lowest DW factor (8%). The total emission efficiency of the remaining candidates also depends on nonradiative relaxation.

HSE06 photoluminescence spectra for neutral $N_{\mathrm{Si}}V_{\mathrm{C}}$, $O_{\mathrm{Si}}V_{\mathrm{C}}$, $P_{\mathrm{Si}}V_{\mathrm{C}}$, and $S_{\mathrm{Si}}V_{\mathrm{C}}$

Figure 3. HSE06 PL spectra for the spin-conserving optical transitions in neutral NSiVCN_{\mathrm{Si}}V_{\mathrm{C}} (a), OSiVCO_{\mathrm{Si}}V_{\mathrm{C}} (b), PSiVCP_{\mathrm{Si}}V_{\mathrm{C}} (c), and SSiVCS_{\mathrm{Si}}V_{\mathrm{C}} (d).

DefectTransition pathTDM (D)ZPL (eV)HRDWτrad\tau_{\mathrm{rad}} (ns)
NSiVCN_{\mathrm{Si}}V_{\mathrm{C}}1b2↑→2b2↑1b_{2}^{\uparrow} \rightarrow2b_{2}^{\uparrow}9.00.620.6552%120.4
OSiVCO_{\mathrm{Si}}V_{\mathrm{C}}1b2↑→2b2↑1b_{2}^{\uparrow} \rightarrow2b_{2}^{\uparrow}5.40.752.538%185.3
PSiVCP_{\mathrm{Si}}V_{\mathrm{C}}1b2↑→2b2↑1b_{2}^{\uparrow} \rightarrow2b_{2}^{\uparrow}9.21.151.3326%18.2
SSiVCS_{\mathrm{Si}}V_{\mathrm{C}}1b2↑→2b2↑1b_{2}^{\uparrow} \rightarrow2b_{2}^{\uparrow}8.11.012.0113%33.5

Table 3 (PDF p. 12). Optical transitions, TDMs, ZPL energies, HR and DW factors, and radiative lifetimes (τrad\tau_{\mathrm{rad}}) of neutral XSiVCX_{\mathrm{Si}}V_{\mathrm{C}} defects (X=NX = \mathrm{N}, O\mathrm{O}, P\mathrm{P}, and S\mathrm{S}). All calculations were performed at the HSE06 level.

Excited-state relaxation can proceed through fluorescence, spin-conserving internal conversion (IC), or intersystem crossing (ISC) between states with different spin multiplicities. We compared the excited-state energies and spin multiplicities of NSiVCN_{\mathrm{Si}}V_{\mathrm{C}}, PSiVCP_{\mathrm{Si}}V_{\mathrm{C}}, and SSiVCS_{\mathrm{Si}}V_{\mathrm{C}} to identify possible competing pathways (Table S3). Fig. S3 shows the orbital occupancies, total spins, and energies relative to S1S_1 for the excited states (SnS_n). All examined excited states of NSiVCN_{\mathrm{Si}}V_{\mathrm{C}} and PSiVCP_{\mathrm{Si}}V_{\mathrm{C}} had doublet character, and no lower-energy excited state was identified. For SSiVCS_{\mathrm{Si}}V_{\mathrm{C}}, a triplet excited state lay 0.145 eV below the optically excited singlet, providing a possible ISC channel. Population in this triplet could subsequently relax through phosphorescence or nonradiative decay.

Figure 4 presents one-dimensional configuration-coordinate diagrams, electron–phonon coupling, and temperature-dependent nonradiative lifetimes for NSiVCN_{\mathrm{Si}}V_{\mathrm{C}}, PSiVCP_{\mathrm{Si}}V_{\mathrm{C}}, and SSiVCS_{\mathrm{Si}}V_{\mathrm{C}}.

One-dimensional configuration-coordinate diagrams, electron–phonon coupling, and temperature-dependent nonradiative lifetimes for the NSiVC, PSiVC, and SSiVC defects

Figure 4. One-dimensional configuration-coordinate diagrams (a–c), electron–phonon coupling (d–f), and temperature-dependent nonradiative lifetimes (g–i) for the NSiVCN_{\mathrm{Si}}V_{\mathrm{C}}, PSiVCP_{\mathrm{Si}}V_{\mathrm{C}}, and SSiVCS_{\mathrm{Si}}V_{\mathrm{C}} defects. Panels (a)–(c) show the ground-state (final) and excited-state (initial) potential-energy surfaces as functions of the mass-weighted configuration coordinate QQ. Symbols denote the calculated energies, and solid curves are parabolic fits used to determine the effective phonon energies ℏΩi\hbar\Omega_i and ℏΩf\hbar\Omega_f. Panels (d)–(f) show the signed wave-function overlaps as functions of QQ. Symbols denote the calculated overlaps, and solid lines are linear fits used to extract the electron–phonon coupling matrix elements WifW_{if}. All calculations were performed at the HSE06 level.

Panels (a)–(c) show the excited- and ground-state potential-energy surfaces along QQ, from which the effective phonon energies ℏΩi\hbar\Omega_i and ℏΩf\hbar\Omega_f were obtained. Linear fits to the signed wave-function overlaps versus QQ in panels (d)–(f) yield WifW_{if}. The parameters ℏΩi\hbar\Omega_i, ℏΩf\hbar\Omega_f, and WifW_{if} enter the expression for the IC-rate in Eq. (7). The reciprocals of the IC rates give the nonradiative lifetimes, shown in panels (g)–(i). These nonradiative lifetimes decreased with increasing temperature, but varied only weakly at low temperatures. For NSiVCN_{\mathrm{Si}}V_{\mathrm{C}}, even the longest nonradiative lifetime, 82.2 ns, was shorter than its radiative lifetime of 120.4 ns. This competition limited its predicted luminescence quantum yield to at most approximately 41%, despite a DW factor of 52%. The HR factor characterizes lattice displacement during the optical transition, whereas IC also depends on electronic coupling and vibrational-state overlap. Weak phonon sidebands therefore do not necessarily imply weak nonradiative decay. For PSiVCP_{\mathrm{Si}}V_{\mathrm{C}}, the nonradiative lifetime remained much longer than the radiative lifetime up to 800 K. This behavior supports a near-unity quantum yield within the model that includes radiative decay and IC. SSiVCS_{\mathrm{Si}}V_{\mathrm{C}} likewise exhibited negligible IC relative to radiative decay, but its lower-energy triplet provides a possible ISC pathway that could reduce its total quantum yield. This possible additional loss channel makes PSiVCP_{\mathrm{Si}}V_{\mathrm{C}} the leading candidate among the investigated defects.

To aid microscopic identification of the four defects, we calculated hyperfine tensors and spin-density distributions. NSiVCN_{\mathrm{Si}}V_{\mathrm{C}} and PSiVCP_{\mathrm{Si}}V_{\mathrm{C}} exhibit strongly anisotropic coupling, as summarized in Table 4. For NSi_{\mathrm{Si}}VC_{\mathrm{C}}, the N hyperfine principal values are (4.2, 4.2, 19.8) MHz.

The strongest Si-site coupling occurs at Si3_3 and Si4_4, with Azz=−87.9A_{zz} = -87.9 MHz, whereas the C-site couplings are comparatively small. PSiVC exhibits stronger on-site coupling at P, with (Axx,Ayy,Azz)=(−60.4,−53.2,121.9)(A_{xx}, A_{yy}, A_{zz}) = (-60.4, -53.2, 121.9) MHz, alongside appreciable coupling to neighboring Si atoms.

These distinct dopant tensors provide microscopic signatures for distinguishing the two spin-active defects.

The positive dopant AzzA_{zz} values and negative values at selected Si sites reflect the combined Fermi-contact and dipolar contributions. These site-resolved hyperfine patterns can help identify constituent atoms and distinguish microscopic models of SiC color centers [4, 25].

OSi_{\mathrm{Si}}VC_{\mathrm{C}} and SSi_{\mathrm{Si}}VC_{\mathrm{C}} have spin-unpolarized (S=0S = 0) ground states, so their ground-state hyperfine tensors vanish within the present approximation.

DefectAtomsAxxA_{xx} (MHz)AyyA_{yy} (MHz)AzzA_{zz} (MHz)
NSi_{\mathrm{Si}}VC_{\mathrm{C}}N4.24.219.8
C1_1, C2_2-11.3-9.5-13.1
C3_3, C4_4-9.1-8.5-13.8
C5_5, C6_6-5.1-2.7-5.6
C7_70.90.73.4
Si1_1, Si2_2-11.9-11.8-41.8
Si3_3, Si4_4-10.0-5.5-87.9
Si5_5-5.1-5.1-26.3
PSiVCP-60.4-53.2121.9

Table 4. HSE06 hyperfine principal values (AxxA_{xx}, AyyA_{yy}, and AzzA_{zz}) for 29^{29}Si, 13^{13}C, 14^{14}N, and 31^{31}P nuclei at the labeled sites in NSi_{\mathrm{Si}}VC_{\mathrm{C}} and PSiVC. Atom labels are defined in Figure 5.

C1_{1}, C2_{2}-1.80.9-3.0
C3_{3}, C4_{4}-6.3-5.7-6.6
C5_{5}, C6_{6}-3.40.5-3.8
C7_{7}1.10.93.4
Si1_{1}, Si2_{2}-5.5-5.2-25.5
Si3_{3}, Si4_{4}-5.8-1.4-65.4
Si5_{5}-2.5-2.4-17.9

Table 4 (PDF p. 17).

Figure 5 shows that the unpaired spin in NSi_{\mathrm{Si}}VC_{\mathrm{C}} and PSi_{\mathrm{Si}}VC_{\mathrm{C}} is localized within the reconstructed defect complex. In both defects, the spin density extends over the dopant and neighboring Si–C framework. This localization is consistent with the defect-state wave functions in Figure 2 and the site-resolved hyperfine tensors. Together, the spin-density distributions and tensor anisotropies provide complementary microscopic signatures for identification by electron paramagnetic resonance (EPR).

HSE06 spin-density distributions of NSiVC and PSiVC in top and side views

Figure 5. HSE06 spin-density distributions of NSi_{\mathrm{Si}}VC_{\mathrm{C}} (a) and PSi_{\mathrm{Si}}VC_{\mathrm{C}} (b) in top and side views. Blue and brown spheres represent Si and C atoms, respectively, while purple and red spheres denote N and P, respectively. Hyperfine constants for the labeled atoms are given in Table 4.

Light-green and yellow lobes represent negative and positive spin-density isosurfaces, respectively, with an absolute isosurface value of 10−3 A˚−310^{-3}\,\mathring{\mathrm{A}}^{-3}.

Conclusion

Our HSE06 calculations identify thermodynamically stable neutral charge states and localized optical transitions in XSiVCX_{\mathrm{Si}}V_{\mathrm{C}} complexes (X = N, O, P, and S) in monolayer SiC. By assessing radiative and nonradiative decay, we find that PSi_{\mathrm{Si}}VC_{\mathrm{C}} is the leading SPE candidate among these complexes. It combines a large TDM (9.2 D) with a short radiative lifetime (18.2 ns) and negligible IC loss up to 800 K, supporting a near-unity quantum yield within the modeled radiative and IC channels. NSi_{\mathrm{Si}}VC_{\mathrm{C}} has the largest DW factor (52%), but multiphonon decay limits its predicted luminescence quantum yield to below 50%. SSi_{\mathrm{Si}}VC_{\mathrm{C}} also exhibits rapid radiative decay and negligible IC, but ISC through a lower-energy triplet could reduce its total quantum yield. Dopant-specific hyperfine tensors and localized spin densities provide experimentally testable signatures for identifying the spin-active NSi_{\mathrm{Si}}VC_{\mathrm{C}} and PSi_{\mathrm{Si}}VC_{\mathrm{C}} defects. Although previous screening studies of SPE candidates have often emphasized radiative metrics such as ZPL energy, transition dipole moment, and DW factor, nonradiative decay can quench emission and limit the quantum efficiency required for quantum applications. Our results establish a joint radiative–nonradiative screening strategy for rational SPE design and identify PSi_{\mathrm{Si}}VC_{\mathrm{C}} as a promising SPE in monolayer SiC.

Acknowledgments

This work was supported by the National Natural Science Foundation of China (Grant No. 12564036, 62674031), the Natural Science Foundation of Jiangxi Province (Grant No. 20252BAC250005), and the Science Challenge Project (Grant No. TZ2025013). The authors acknowledge the Hefei Advanced Computing Center for computational resources.

AUTHOR DECLARATIONS

Conflict of Interest

The authors declare no conflicts of interest.

DATA AVAILABILITY

The data supporting the findings of this study are available from the corresponding authors upon reasonable request.

References

  1. [1]I. Aharonovich, D. Englund, and M. Toth, Solid-state single-photon emitters, Nat. Photon. 10, 631 (2016).DOI
  2. [2]G. Wolfowicz, F. J. Heremans, C. P. Anderson, S. Kanai, H. Seo, A. Gali, G. Galli, and D. D. Awschalom, Quantum guidelines for solid-state spin defects, Nat. Rev. Mater. 6, 906 (2021).DOI
  3. [3]N. Lo Piparo, M. Razavi, and W. J. Munro, Memory-assisted quantum key distribution with a single nitrogen-vacancy center, Phys. Rev. A 96, 052313 (2017).DOI
  4. [4]N. T. Son, C. P. Anderson, A. Bourassa, K. C. Miao, C. Babin, M. Widmann, M. Niethammer, J. Ul Hassan, N. Morioka, I. G. Ivanov, F. Kaiser, J. Wrachtrup, and D. D. Awschalom, Developing silicon carbide for quantum spintronics, Appl. Phys. Lett. 116, 190501 (2020).DOI
  5. [5]G. Balasubramanian, I. Y. Chan, R. Kolesov, M. Al-Hmoud, J. Tisler, C. Shin, C. Kim, A. Wojcik, P. R. Hemmer, A. Krueger, T. Hanke, A. Leitenstorfer, R. Bratschitsch, F. Jelezko, and J. Wrachtrup, Nanoscale imaging magnetometry with diamond spins under ambient conditions, Nature 455, 648 (2008).DOI
  6. [6]P. Li, J.-Y. Zhou, S. Li, P. Udvarhelyi, J.-S. Xu, C.-F. Li, B. Huang, G.-C. Guo, and A. Gali, Non-invasive bioinert room-temperature quantum sensor from silicon carbide qubits, Nat. Mater. 24, 1913 (2025).DOI
  7. [7]C. L. Degen, F. Reinhard, and P. Cappellaro, Quantum sensing, Rev. Mod. Phys. 89, 035002 (2017).DOI
  8. [8]N. Mendelson, D. Chugh, J. R. Reimers, T. S. Cheng, A. Gottscholl, H. Long, C. J. Mellor, A. Zettl, V. Dyakonov, P. H. Beton, S. V. Novikov, C. Jagadish, H. H. Tan, M. J. Ford, M. Toth, C. Bradac, and I. Aharonovich, Identifying carbon as the source of visible single-photon emission from hexagonal boron nitride, Nat. Mater. 20, 321 (2021).
  9. [9]G. Kucksko, P. C. Maurer, N. Y. Yao, M. Kubo, H. J. Noh, P. K. Lo, H. Park, and M. D. Lukin, Nanometre-scale thermometry in a living cell, Nature 500, 54 (2013).
  10. [10]M. W. Doherty, F. Dolde, H. Fedder, F. Jelezko, J. Wrachtrup, N. B. Manson, and L. C. L. Hollenberg, Theory of the ground-state spin of the NV⁻ center in diamond, Phys. Rev. B 85, 205203 (2012).DOI
  11. [11]G. Balasubramanian, P. Neumann, D. Twitchen, M. Markham, R. Kolesov, N. Mizuochi, J. Isoya, J. Achard, J. Beck, J. Tissler, V. Jacques, P. R. Hemmer, F. Jelezko, and J. Wrachtrup, Ultralong spin coherence time in isotopically engineered diamond, Nat. Mater. 8, 383 (2009).DOI
  12. [12]L. Childress and R. Hanson, Diamond NV centers for quantum computing and quantum networks, MRS Bull. 38, 134 (2013).DOI
  13. [13]J. R. Maze, A. Gali, E. Togan, Y. Chu, A. Trifonov, E. Kaxiras, and M. D. Lukin, Properties of nitrogen-vacancy centers in diamond: the group theoretic approach, New J. Phys. 13, 025025 (2011).DOI
  14. [14]C. Bradac, W. Gao, J. Forneris, M. E. Trusheim, and I. Aharonovich, Quantum nanophotonics with group IV defects in diamond, Nat. Commun. 10, 5625 (2019).
  15. [15]L. J. Rogers, K. D. Jahnke, T. Teraji, L. Marseglia, C. Müller, B. Naydenov, H. Schauffert, C. Kranz, J. Isoya, L. P. McGuinness, and F. Jelezko, Multiple intrinsically identical single-photon emitters in the solid state, Nat. Commun. 5, 4739 (2014).DOI
  16. [16]D. D. Sukachev, A. Sipahigil, C. T. Nguyen, M. K. Bhaskar, R. E. Evans, F. Jelezko, and M. D. Lukin, Silicon-Vacancy Spin Qubit in Diamond: A Quantum Memory Exceeding 10 ms with Single-Shot State Readout, Phys. Rev. Lett. 119, 223602 (2017).DOI
  17. [17]X. Guo, A. M. Stramma, Z. Li, W. G. Roth, B. Huang, Y. Jin, R. A. Parker, J. Arjona Martínez, N. Shofer, C. P. Michaels, C. P. Purser, M. H. Appel, E. M. Alexeev, T. Liu, A. C. Ferrari, D. D. Awschalom, N. Delegan, B. Pingault, G. Galli, F. J. Heremans, M. Atatüre, and A. A. High, Microwave-Based Quantum Control and Coherence Protection of Tin-Vacancy Spin Qubits in a Strain-Tuned Diamond-Membrane Heterostructure, Phys. Rev. X 13, 041037 (2023).
  18. [18]T. Iwasaki, Y. Miyamoto, T. Taniguchi, P. Siyushev, M. H. Metsch, F. Jelezko, and M. Hatano, Tin-Vacancy Quantum Emitters in Diamond, Phys. Rev. Lett. 119, 253601 (2017).
  19. [19]X. Cheng, A. Thurn, G. Chen, G. S. Jones, J. E. Bennett, M. Coke, M. Adshead, C. P. Michaels, O. Balci, A. C. Ferrari, M. Atatüre, R. J. Curry, J. M. Smith, P. S. Salter, and D. A. Gangloff, Laser activation of single group-IV colour centres in diamond, Nat. Commun. 16, 5124 (2025).
  20. [20]G. Thiering and A. Gali, Ab Initio Magneto-Optical Spectrum of Group-IV Vacancy Color Centers in Diamond, Phys. Rev. X 8, 021063 (2018).
  21. [21]R. Bai, D. Liu, S. Chen, and Y.-N. Wu, Origin of the unidentified color centers in $4H$-SiC from first principles, Phys. Rev. B 111, 014106 (2025).DOI
  22. [22]S. Castelletto, B. C. Johnson, V. Ivady, N. Stavrias, T. Umeda, A. Gali, and T. Ohshima, A silicon carbide room-temperature single-photon source, Nat. Mater. 13, 151 (2014).DOI
  23. [23]R.-Z. Fang, X.-Y. Lai, T. Li, R.-Z. Su, B.-W. Lu, C.-W. Yang, R.-Z. Liu, Y.-K. Qiao, C. Li, Z.-G. He, J. Huang, H. Li, L.-X. You, Y.-H. Huo, X.-H. Bao, and J.-W. Pan, Experimental Generation of Spin-Photon Entanglement in Silicon Carbide, Phys. Rev. Lett. 132, 160801 (2024).DOI
  24. [24]M. Mohseni, P. Udvarhelyi, G. Thiering, and A. Gali, Positively charged carbon vacancy defect as a near-infrared emitter in 4H-SiC, Phys. Rev. Mater. 7, 096202 (2023).arxiv.org/abs/2305.17483
  25. [25]A. Lohrmann, B. C. Johnson, J. C. McCallum, and S. Castelletto, A review on single photon sources in silicon carbide, Rep. Prog. Phys. 80, 034502 (2017).DOI
  26. [26]S. Gupta, W. Wu, S. Huang, and B. I. Yakobson, Single-Photon Emission from Two-Dimensional Materials, to a Brighter Future, J. Phys. Chem. Lett. 14, 3274 (2023).DOI
  27. [27]F. Peyskens, C. Chakraborty, M. Muneeb, D. Van Thourhout, and D. Englund, Integration of single photon emitters in 2D layered materials with a silicon nitride photonic chip, Nat. Commun. 10, 4435 (2019).
  28. [28]S. Wang, X. Liu, M. Xu, L. Liu, D. Yang, and P. Zhou, Two-dimensional devices and integration towards the silicon lines, Nat. Mater. 21, 1225 (2022).DOI
  29. [29]A. Sajid, M. J. Ford, and J. R. Reimers, Single-photon emitters in hexagonal boron nitride: a review of progress, Rep. Prog. Phys. 83, 044501 (2020).DOI
  30. [30]T. T. Tran, K. Bray, M. J. Ford, M. Toth, and I. Aharonovich, Quantum emission from hexagonal boron nitride monolayers, Nat. Nanotechnol. 11, 37 (2016).
  31. [31]T. T. Tran, C. Elbadawi, D. Totonijian, C. J. Lobo, G. Grosso, H. Moon, D. R. Englund, M. J. Ford, I. Aharonovich, and M. Toth, Robust Multicolor Single Photon Emission from Point Defects in Hexagonal Boron Nitride, ACS Nano 10, 7331 (2016).arxiv.org/abs/1603.09608
  32. [32]B. Whitefield, H. Z. J. Zeng, J. Liddle-Wesolowski, I. O. Robertson, Á. Ganyecz, V. Ivady, K. Watanabe, T. Taniguchi, M. Toth, J.-P. Tetienne, I. Aharonovich, and M. Kianinia, Narrowband quantum emitters in hexagonal boron nitride with optically addressable spins, Nat. Mater. 25, 412 (2026).DOI
  33. [33]H. L. Stern, C. M. Gilardoni, Q. Gu, S. Eizagirre Barker, O. F. J. Powell, X. Deng, S. A. Fraser, L. Follet, C. Li, A. J. Ramsay, H. H. Tan, I. Aharonovich, and M. Atatüre, A quantum coherent spin in hexagonal boron nitride at ambient conditions, Nat. Mater. 23, 1379 (2024).
  34. [34]C. Cholsuk, S. Suwanna, and T. Vogl, Comprehensive Scheme for Identifying Defects in Solid-State Quantum Systems, J. Phys. Chem. Lett. 14, 6564 (2023).DOI
  35. [35]M. Mackoit-Sinkevičienė, M. Maciaszek, C. G. Van de Walle, and A. Alkauskas, Carbon dimer defect as a source of the 4.1 eV luminescence in hexagonal boron nitride, Appl. Phys. Lett. 115, 212101 (2019).
  36. [36]Y. Lee, Y. Hu, X. Lang, D. Kim, K. Li, Y. Ping, K. C. Fu, and K. Cho, Spin-defect qubits in two-dimensional transition metal dichalcogenides operating at telecom wavelengths, Nat. Commun. 13, 7501 (2022).DOI
  37. [37]A. Singh and A. K. Singh, A typical behavior of intrinsic defects and promising dopants in two-dimensional WS₂, Phys. Rev. Mater. 5, 084001 (2021).DOI
  38. [38]M. Koperski, K. Nogaijewski, A. Arora, V. Cherkez, P. Mallet, J. Y. Veuillen, J. Marcus, P. Kossacki, and M. Potemski, Single photon emitters in exfoliated WSe₂ structures, Nat. Nanotechnol. 10, 503 (2015).DOI
  39. [39]Y.-M. He, G. Clark, J. R. Schaibley, Y. He, M.-C. Chen, Y.-J. Wei, X. Ding, Q. Zhang, W. Yao, X. Xu, C.-Y. Lu, and J.-W. Pan, Single quantum emitters in monolayer semiconductors, Nat. Nanotechnol. 10, 497 (2015).DOI
  40. [40]S. Li, G. Thiering, P. Udvarhelyi, V. Ivády, and A. Gali, Carbon defect qubit in two-dimensional WS2, Nat. Commun. 13, 1210 (2022).DOI
  41. [41]J.-Y. Tsai, J. Pan, H. Lin, A. Bansil, and Q. Yan, Antisite defect qubits in monolayer transition metal dichalcogenides, Nat. Commun. 13, 492 (2022).DOI
  42. [42]J. C. Thomas, W. Chen, Y. Xiong, B. A. Barker, J. Zhou, W. Chen, A. Rossi, N. Kelly, Z. Yu, D. Zhou, S. Kumari, E. S. Barnard, J. A. Robinson, M. Terrones, A. Schwartzberg, D. F. Ogletree, E. Rotenberg, M. M. Noack, S. Griffin, A. Raja, D. A. Strubbe, G.-M. Rignanese, A. Weber-Bargioni, and G. Hautier, A substitutional quantum defect in WS2 discovered by high-throughput computational screening and fabricated by site-selective STM manipulation, Nat. Commun. 15, 3556 (2024).DOI
  43. [43]J. Huang, B. Huang, and S. Li, Dimensionality-Driven Charge Stabilization of Group-IV Color Centers in Diamond Ultrathin Films, Nano Lett. 26, 14656 (2026).arxiv.org/abs/2606.08550
  44. [44]J. Lee, H. Wang, K.-Y. Park, S. Huh, D. Kim, M. Yu, C. Kim, K. S. Thygesen, and J. Lee, Room Temperature Quantum Emitters in van der Waals α-MoO3, Nano Lett. 25, 1142 (2025).DOI
  45. [45]S. Chabi, Z. Guler, A. J. Brearley, A. D. Benavidez, and T. S. Luk, The Creation of True Two-Dimensional Silicon Carbide, Nanomaterials 11, 1799 (2021).DOI
  46. [46]C. M. Polley, H. Fedderwitz, T. Balasubramanian, A. A. Zakharov, R. Yakimova, O. Backe, J. Ekman, S. P. Dash, S. Kubatkin, and S. Lara-Avila, Bottom-Up Growth of Monolayer Honeycomb SiC, Phys. Rev. Lett. 130, 076203 (2023).DOI
  47. [47]Q. Hassanzada, I. A. Sarsari, A. Hashemi, A. Ghojavand, A. Gali, and M. Abdi, Theoretical study of quantum emitters in two-dimensional silicon carbide monolayers, Phys. Rev. B 102, 134103 (2020).DOI
  48. [48]M. Mohseni, I. A. Sarsari, S. Karbasizadeh, P. Udvarhelyi, Q. Hassanzada, T. Ala-Nissila, and A. Gali, Vacancy-related color centers in two-dimensional silicon carbide monolayers, Phys. Rev. Mater. 8, 056201 (2024).
  49. [49]J. Huang, Q. Ke, and X. Lei, First-principles investigation of point defects in two-dimensional SiC as single-photon sources, Phys. Rev. B 112, 085303 (2025).DOI
  50. [50]J. Huang, Q. Ke, and X. Lei, First-principles prediction of spin-triplet qubits in two-dimensional silicon carbide, Phys. Rev. B 112, 205303 (2025).DOI
  51. [51]S. Li, A. Gali, and B. Huang, Computation-aided design of color centers for quantum information processing, Newton 2, 100432 (2026).DOI
  52. [52]G. Zhang, Y. Cheng, J.-P. Chou, and A. Gali, Material platforms for defect qubits and single-photon emitters, Appl. Phys. Rev. 7, 031308 (2020).arxiv.org/abs/2008.06458
  53. [53]G. Kresse and J. Hafner, Ab initio molecular dynamics for liquid metals, Phys. Rev. B 47, 558 (1993).
  54. [54]G. Kresse and J. Furthmüller, Efficient iterative schemes for ab initio total-energy calculations using a plane-wave basis set, Phys. Rev. B 54, 11169 (1996).pubmed.ncbi.nlm.nih.gov/9984901
  55. [55]P. E. Blöchl, Projector augmented-wave method, Phys. Rev. B 50, 17953 (1994).pubmed.ncbi.nlm.nih.gov/9976227
  56. [56]G. Kresse and D. Joubert, From ultrasoft pseudopotentials to the projector augmented-wave method, Phys. Rev. B 59, 1758 (1999).DOI
  57. [57]J. P. Perdew, K. Burke, and M. Ernzerhof, Generalized Gradient Approximation Made Simple, Phys. Rev. Lett. 77, 3865 (1996).pubmed.ncbi.nlm.nih.gov/10062328
  58. [58]J. Heyd, G. E. Scuseria, and M. Ernzerhof, Hybrid functionals based on a screened Coulomb potential, J. Chem. Phys. 118, 8207 (2003).DOI
  59. [59]P. Deák, B. Aradi, T. Frauenheim, E. Janzén, and A. Gali, Accurate defect levels obtained from the HSE06 range-separated hybrid functional, Phys. Rev. B 81, 153203 (2010).DOI
  60. [60]H. J. Monkhorst and J. D. Pack, Special points for Brillouin-zone integrations, Phys. Rev. B 13, 5188 (1976).DOI
  61. [61]A. Togo and I. Tanaka, First principles phonon calculations in materials science, Scripta Mater. 108, 1 (2015).arxiv.org/abs/1506.08498
  62. [62]A. Gali, E. Janzén, P. Deák, G. Kresse, and E. Kaxiras, Theory of Spin-Conserving Excitation of the N-V- Center in Diamond, Phys. Rev. Lett. 103, 186404 (2009).DOI
  63. [63]C. Freysoldt and J. Neugebauer, First-principles calculations for charged defects at surfaces, interfaces, and two-dimensional materials in the presence of electric fields, Phys. Rev. B 97, 205425 (2018).DOI
  64. [64]See https://sxrepo.mpie.de.
  65. [65]V. Wang, N. Xu, J.-C. Liu, G. Tang, and W.-T. Geng, VASPkit: A user-friendly interface facilitating high-throughput computing and analysis using VASP code, Comput. Phys. Commun. 267, 108033 (2021).
  66. [66]S. A. Tawfik and S. P. Russo, PyPhotonics: A python package for the evaluation of luminescence properties of defects, Comput. Phys. Commun. 273, 108222 (2022).DOI
  67. [67]S. Li and A. Gali, Identification of an Oxygen Defect in Hexagonal Boron Nitride, J. Phys. Chem. Lett. 13, 9544 (2022).DOI
  68. [68]M. E. Turiansky, A. Alkauskas, M. Engel, G. Kresse, D. Wickramaratne, J.-X. Shen, C. E. Dreyer, and C. G. Van de Walle, Nonrad: Computing nonradiative capture coefficients from first principles, Comput. Phys. Commun. 267, 108056 (2021).

Paper details

vlnc:W_vjq8gdy4
Version
v1 · latest
Published
Fresh — added to the Hub within the last 30 days
Added
License
CC BY 4.0
Usage

views · 0

downloads · 0

A view counts once per browser per day, a download each time the PDF is requested.

  • Physics and Astronomy

Not recorded for this paper

View statement
Looking for related papers…
Contents