Origin of Bright Quantum Emissions with High Debye-Waller factor in Silicon Nitride

Abstract

Silicon nitride has emerged as a promising photonic platform for integrated single-photon sources, yet the microscopic origin of the recently observed bright quantum emissions remains unclear. Using hybrid density functional theory, we show that the negatively charged NSi_\text{Si}VN_\text{N} center (NV−^{-}) in the C1h_{1h} configuration exhibits a linearly polarized zero-phonon line (ZPL) at 2.46 eV, with a radiative lifetime of 9.01 ns and a high Debye-Waller (DW) factor of 33%. We further find that the C1h_{1h} configuration is prone to a pseudo-Jahn-Teller distortion, yielding two symmetrically equivalent defect structures that emit bright, linearly polarized ZPL at 1.80 eV with a lifetime of 10.17 ns and an increased DW factor of 41%. These nitrogen-vacancy-related defects explain the origins of visible quantum emissions, paving the way for deterministic and monolithically integrated silicon-nitride quantum photonics.

Bright single-photon emitters operating near the visible spectrum have attracted significant interest, exemplified by the ∼2\sim2 eV emitter in hBN [1] and the NV−\mathrm{NV}^{-} center in diamond [2]. Hybrid integration approaches, which combine different materials for the emission source and photonic elements, increase fabrication complexity and introduce coupling losses at interfaces [1, 3]. A unified photonic platform with built-in single-photon emitters is therefore crucial for achieving direct, scalable, and low-loss integration of quantum light sources. Silicon nitride has emerged as a state-of-the-art quantum photonic platform, offering a wide bandgap suitable for hosting quantum emitters. Recently, room-temperature single-photon emissions near ∼2\sim2 eV have been observed in silicon nitride [3, 4]. These emitters are bright, stable, linearly polarized, and exhibit high purity. Most importantly, monolithic integration of these emitters within the silicon nitride photonic platform has been demonstrated [5]. However, the microscopic origin of these emitters remains unidentified.

Senichev et al. [4] reported intrinsic single-photon emitters in silicon nitride, emitting in the range of 568-722 nm (2.18-1.72 eV) at room temperature. Using a similar synthesis procedure, Martin et al. [3] observed several emitters with ZPL emission around 548 nm (2.26 eV) with a 7 nm deviation at 4.2 K. In both studies, silicon nitride films were grown under nitrogen-rich conditions on SiO2_2/Si substrates. Analysis of 130 emitters revealed an average second-order autocorrelation value of 0.2 at zero delay, confirming high single-photon purity. Fluorescence lifetime measurements under pulsed excitation for 44 emitters yielded lifetimes ranging from 1.4 to 3.9 ns, with an average of 2.4 ns. The emitters exhibited bright and stable emission without noticeable blinking or bleaching for up to 100 s at saturation power. More recently, Chen et al. [6] identified single-photon emitters with emission between 570 and 582 nm (2.18-2.13 eV), showing large Debye-Waller factors (50-74%) and lifetimes of 3-8 ns. These emitters were attributed to defects in the silica substrate, despite being synthesized using the same method as in Refs. [3, 4]. Given these consistent optical signatures yet differing interpretations, identifying the microscopic nature of these quantum emitters is essential for enabling targeted quantum-optics measurements and deterministic defect creation in integrated Si3_3N4_4 photonic platforms.

In this letter, we identify the microscopic origin of the ∼2\sim2 eV single-photon emitters observed in silicon nitride. Using hybrid density-functional theory, we investigate the thermodynamic stability, electronic structure, and optical properties of the nitrogen-vacancy-antisite (NSiVNN_{\mathrm{Si}}V_{\mathrm{N}}, or NV center) defect in β\beta-Si3_3N4_4. We show that this defect exhibits a bright, linearly polarized optical emission whose ZPL, radiative lifetime, and DW factor are in close agreement with experimentally reported emitter characteristics. We further reveal that a pseudo-Jahn-Teller distortion creates additional symmetry-broken configurations that remain optically active and fall within the same spectral window.

β\beta-Si3_3N4_4 crystallizes in the centrosymmetric P63_3/m space group [7], with two inequivalent nitrogen sites (C3h_{3h} and mm) and a single silicon site of mm symmetry. In this work, we consider the nitrogen vacancy at the C3h_{3h} site (VN_{\mathrm{N}}) and the associated nitrogen-antisite-vacancy complex (NSi_{\mathrm{Si}}VN_{\mathrm{N}}). Defects are modeled in a 280-atom hexagonal supercell with Γ\Gamma-point sampling of the brillouin zone. Calculations are performed using the hybrid Heyd-Scuseria-Ernzerhof (HSE) functional [8] and projector augmented-wave potentials [9], as implemented in VASP [10]. A Hartree-Fock exchange fraction of α=0.30\alpha= 0.30 yields a band gap of 6.1 eV, in good agreement with experiment [1] [see Sec. S1 of the Supplementary Information (SI); see also Refs. [1, 2, 3, 4, 16] [5, 7, 8, 9, 10] therein]. Unit-cell optimizations used a 4×4×44 \times4 \times4 Monkhorst-Pack k-mesh [21] and a 400 eV plane-wave cutoff, giving relaxed lattice constants a=b=7.61a=b=7.61 Å and c=2.91c=2.91 Å, consistent with Ref. [22]. Furthermore, the calculated formation enthalpy of -8.96 eV per formula unit is in good agreement with that of the experimentally reported value of -8.58 eV [23]. Supercell geometries were relaxed using PBE functional [24] until forces were below 0.001 eV/Å, followed by electronic structure calculation using hybrid-functional. Excited-state energies and geometries were obtained using the Δ\DeltaSCF method [25] and spin polarization is explicitly considered in all the calculations. Electron-phonon coupling was analyzed using PHONOPY [26] and DEFECTPL [27, 28] [7]. Finite-size corrections for charged defects were applied using the eFNV scheme [3] via DOPED [4]. Further computational details are provided in § 3 of SI.

From defect formation energy calculations, we find that the nitrogen vacancy (VNV_{\mathrm{N}}) is the most stable intrinsic defect in β\beta-Si3_3N4_4, consistent with previous computational and experimental studies [29, 30]. As shown in Figure 1(a) and Figure S1 in the SI, VNV_{\mathrm{N}} exhibits the lowest formation energy under both nitrogen-rich and silicon-rich conditions. The nitrogen-rich growth environments employed in recent experiments [3, 4, 6] also favor the formation of stable NSiN_{\mathrm{Si}} defects. Furthermore, thermal annealing used to activate the emitters [4] can promote migration of NSiN_{\mathrm{Si}} and VNV_{\mathrm{N}}, enabling NV center formation throughout the Si3_3N4_4 matrix. Our nudged elastic band calculations suggest that the formation of the NSiVNN_{\mathrm{Si}}V_{\mathrm{N}} defect from VSi−V_{\mathrm{Si}}^{-} involves a high migration barrier of 2.66 eV, as shown in Figure S4 of the SI. Unlike the NV center in diamond, which constitutes an extrinsic substitutional nitrogen adjacent to a carbon vacancy, the NV defect in β\beta-Si3_3N4_4 originates from an intrinsic nitrogen antisite (NSiN_{\mathrm{Si}}) adjacent to VNV_{\mathrm{N}} [Figure 1(b)]. As shown in Figure 1(a), the NV center is stable in charge states +2 to −2 within the bandgap as the Fermi level varies between the valence band maximum (VBM) and conduction band minimum (CBM). The neutral NV center (NV0^{0}) has a singlet ground state, whereas the charged NV+^{+} and NV−^{-} defects exhibit doublet ground states, each hosting a single unpaired electron. In contrast, the VN0V_{\mathrm{N}}^{0} is paramagnetic with one unpaired electron, while its positive and negative charge states exhibit singlet ground states.

Formation energies and geometry of the nitrogen antisite-vacancy complex

Figure 1. (a) Formation energy of nitrogen vacancy (VNV_{\mathrm{N}}, grey), nitrogen antisite (NSiN_{\mathrm{Si}}, red), and nitrogen antisite-vacancy complex (NSiVNN_{\mathrm{Si}}V_{\mathrm{N}}, green) under N-rich growth conditions. The slopes and kinks in the plot represent the charge states and charge transition levels, respectively. (b) Geometry of the NSiVNN_{\mathrm{Si}}V_{\mathrm{N}} complex, shown along the c-axis projection. Blue, silver, and red atoms represent silicon, nitrogen, and nitrogen-antisite, respectively.

Formation energies of nitrogen vacancy, nitrogen antisite, and nitrogen antisite-vacancy defects in Si-rich growth conditions

Figure S1. Formation energy of nitrogen vacancy, nitrogen antisite, and nitrogen antisite-vacancy defects in Si-rich growth conditions.

Migration barrier from $N_{\mathrm{Si}}V_{\mathrm{N}}^{-}$ to $V_{\mathrm{Si}}^{-}$ and vice-versa

Figure S4. Migration barrier from NSiVN−N_{\mathrm{Si}}V_{\mathrm{N}}^{-} to VSi−V_{\mathrm{Si}}^{-} and vice-versa.

The relaxed geometry of VNV_{\mathrm{N}} exhibits C3hC_{3h} point-group symmetry, in contrast to the C3vC_{3v} symmetry reported by Nanataki et al. [31]. In the neutral charge state, the defect hosts a single unpaired electron occupying a pair of nearly degenerate majority-spin orbitals, which drives a strong Jahn-Teller (JT) distortion of the local environment. In the high-symmetry configuration, the three neighboring Si atoms form an almost perfect equilateral triangle with C3hC_{3h} symmetry. Upon JT distortion, however, this triangle becomes scalene, and the symmetry is lowered to C1hC_{1h}. The resulting symmetry breaking lifts the degeneracy of the defect orbitals and produces a large splitting of approximately 2.9 eV (see Figure S2 in the SI). In contrast, the positively and negatively charged VNV_{\mathrm{N}} states do not exhibit a JT instability and therefore preserve C3hC_{3h} symmetry. When a nitrogen atom substitutes a neighboring Si site, forming the NSiVNN_{\mathrm{Si}}V_{\mathrm{N}} complex, structural relaxation yields a C1hC_{1h} configuration. This structure contains a mirror plane passing through the substituted N atom and the two adjacent Si atoms.

Localized states formed inside the bandgap of $\beta$-Si$_3$N$_4$; Kohn-Sham levels of neutral $V_\mathrm{N}$ defects in major and minor spin channels, with localized wave functions shown at right

Figure S2. Localized states formed inside the bandgap of β\beta-Si3_3N4_4. The left panel shows Kohn-Sham levels of neutral VNV_\mathrm{N} defects in both spin channels within the bandgap. The Fermi level is shown on the vertical axis with values referenced to the valence band maximum. The irreducible representations of localized KS levels are indicated according to the C1hC_{1h} point group symmetry of the defect. The right panel shows the real part of the wave function of the highest occupied (solid border) and lowest unoccupied (dashed border) localized levels. The red line represents the mirror plane symmetry element perpendicular to the c-axis.

Nitrogen vacancy introduces three planar dangling bonds derived from the 3s and 3p orbitals of the neighboring Si atoms. Their interaction produces localized Kohn-Sham (KS) levels within the bandgap (see Figure S2 in the SI). When a nitrogen atom substitutes a nearby Si site to form the NSiVNN_{\mathrm{Si}}V_{\mathrm{N}} center, hybridization between the substituted and surrounding N atoms alters the KS levels. The negatively charged defect features an occupied KS level a′(1)a'(1) just above the VBM and an unoccupied level a′(2)a'(2) located 3.94 eV higher in energy [see C1hC_{1h} configuration in Figure 2(a)]. In the NV−^{-} charge state, these two localized states transform as A′A' irreducible representations, denoted as a′(1)a'(1) (occupied) and a′(2)a'(2) (unoccupied). Both the ground and excited states are spin doublets and represented as 2A′^{2}A'. Optical transitions between them are linearly polarized in the xyxy-plane, producing a ZPL at 2.46 eV with a transition dipole moment (see Eq. (16) in SI) of 4.7 Debye. This is in close agreement with the experimentally reported ZPL near 2.26 eV [3, 4]. The corresponding radiative rate and lifetime (see Eq. (15) in SI) are 111 MHz and 9.01 ns, respectively. Our calculated values also agree well with ZPL (∼\sim2.15 eV) and lifetime (3–8 ns) reported by Chen et al. [6]. Similar nitrogen antisite-vacancy complex defect has also been observed as source of ∼\sim2 eV SPE in GaN [32]. In the majority-spin channel [Figure 2 (a)], the occupied a′a' and unoccupied a′′a'' states give rise to a second dipole-allowed transition polarized along zz, as only ⟨a′∣z∣a′′⟩\langle a'|z|a''\rangle transforms as A′A'. This transition yields a ZPL at 0.85 eV, within the telecommunication spectral range, with a transition dipole of 7.2 Debye and a radiative rate and lifetime of 10.5 MHz and 95.24 ns, respectively.

Defect-level diagram of the NV− center and schematic potential energy surfaces

Figure 2. (a) Defect-level diagram of the NV−^{-} center in the C1h_{1h} configuration (left) and the pseudo-Jahn-Teller (PJT) distorted configuration (C1h_{1h}-PJT, right). Energies are referenced to the valence band maximum (VBM). Red markers indicate Kohn-Sham levels, with a grey arrow denoting the transition from the occupied level [a′(1)a^{\prime}(1)] to the unoccupied level [a′(2)a^{\prime}(2)]. In the C1h_{1h}-PJT configuration, the localized KS levels are labeled as a(1)a(1) and a(2)a(2) due to the absence of symmetry elements, and a blue arrow indicates the transition between them. Isosurfaces of the real part (30% of the maximum) of the wave functions corresponding to occupied and unoccupied levels in the minority-spin channel are shown. (b) Schematic potential energy surfaces (PES) for the ground state (GS, green) and excited state (ES, orange). The PES nodes represent the symmetric ground state (G1), distorted ground states (G2 and G3), and corresponding excited states (E1, E2, and E3). The phonon mode (red arrows) responsible for the distortion from C1h_{1h} (G1) to C1h_{1h}-PJT configurations (G2 and G3) is illustrated. The energy differences between configurations are: ΔEG1−G2=1.00\Delta E_{\mathrm{G1-G2}} = 1.00 eV, ΔEE1−E2=1.66\Delta E_{\mathrm{E1-E2}} = 1.66 eV, ΔEE1−G1=2.46\Delta E_{\mathrm{E1-G1}} = 2.46 eV, and ΔEE2−G2=1.80\Delta E_{\mathrm{E2-G2}} = 1.80 eV. The changes in configuration coordinate are: ΔQG1−G2=2.53\Delta Q_{\mathrm{G1-G2}} = 2.53 amu1/2^{1/2}Å, ΔQE1−E2=2.63\Delta Q_{\mathrm{E1-E2}} = 2.63 amu1/2^{1/2}Å, ΔQE1−G1=0.44\Delta Q_{\mathrm{E1-G1}} = 0.44 amu1/2^{1/2}Å, and ΔQE2−G2=0.36\Delta Q_{\mathrm{E2-G2}} = 0.36 amu1/2^{1/2}Å.

The NV−^{-} center in the C1hC_{1h} configuration exhibits an imaginary phonon mode. This mode corresponds to a localized out-of-plane oscillation of the substituted nitrogen (NSiN_{\mathrm{Si}}) between neighboring nitrogen atoms [Fig. 2(b)], indicating that the C1h_{1h} configuration is an unstable saddle point in the potential energy surface. It originates from the shorter N-N bond compared to the Si-N bond. A small displacement along this mode drives the system toward a lower-symmetry configuration, in which the substituted nitrogen moves closer to one neighboring nitrogen, breaking the mirror symmetry [see Figure 2(b) and Fig. S7 in SI]. Since the C1h_{1h} configuration is nondegenerate yet still distorts, this behavior is classified as a pseudo-Jahn-Teller (PJT) effect [33]. This distortion results in C1_1 point group symmetry and is denoted as C1h_{1h}-PJT from now onwards [Fig. 2(b)]. The two possible distortions, toward either neighboring nitrogen, are energetically degenerate, with approximately 1 eV lower energy than the high-symmetry C1h_{1h} structure. The distortion of the C1h_{1h} configuration of the NV−^{-} defect modifies the energy and symmetry of the localized states [see Fig. 2(a)], altering its optical properties. In the minority-spin channel, C1h_{1h}-PJT configuration exhibits a ZPL at 1.80 eV

and a radiative lifetime of 10.17 ns, in close agreement with experimental reports [4]. In realistic samples, the NV−^{-} center may experience diverse local environments, such as those near interfaces or regions under strain, that can alter its electronic and optical characteristics. Given that the optical response is sensitive to subtle changes in the atomic configuration, as illustrated by the differences in properties of the C1h_{1h} and C1h_{1h}-PJT structures, such local variations likely contribute to the spread and variability observed in experimental measurements.

Next, we analyzed the electron-phonon coupling of this transition using the method of Alkauskas et al. [16]. The photoluminescence spectra show a phonon sideband with three peaks, also reflected in the calculated electron-phonon spectral function [Fig. 3]. The 87 meV phonon mode with the largest partial Huang-Rhys (HR) factor is quaslocalized with a localization ratio of 14.4, while the spectral peaks arise from multiple phonon modes with different degrees of localization [see Fig. 3 and Fig. S3 in SI]. The first peak near 55 meV agrees with the first peak of phonon sideband in the range 38.6-57.4 meV observed in experiment [6], with additional peaks at 83 and 118 meV. The total HR factor is 0.9, corresponding to a DW factor of 41%, which is close to the experimentally measured range of 50-70% reported by Chen et al. [6]. These DW values are significantly higher than the DW factor of 3% for the well-known NV−^{-} center in diamond, even though the ZPL energy and excited-state lifetime are comparable, at approximately ∼2\sim2 eV and 12 ns [34, 35]. The moderate electron-phonon interaction (HR factor = 0.9) ensures that a large fraction of the optical emission remains in the zero-phonon line [see Figure 3(b)]. This behavior arises because the structural relaxation between the ground and excited states is relatively small, with a change in configuration coordinate [ΔQ\Delta Q, see Eq. (11) in SI] of only 0.36 amu1/2^{1/2}Å. For the C1hC_{1h} configuration, the HR and DW factors are 1.11 and 33%, respectively. The strength of the electron-phonon coupling, expressed by the HR factor, is reflected in the calculated ΔQ\Delta Q for both the C1hC_{1h} (0.44 amu1/2^{1/2}Å) and C1hC_{1h}-PJT (0.36 amu1/2^{1/2}Å) geometries. We note that PBE functional underestimates the ground-to-excited state configurational displacement ΔQ\Delta Q relative to that calculated from HSE functional [36], leading to reduced HR factor and overestimated Debye-Waller values. While SCAN provides an improvement over PBE, it still underestimates experimental HR values for the NV−^{-} center in diamond [37]. Thus, our reported HR values represent a reliable lower bound. Earlier studies [3, 4] proposed that the observed photoluminescence features might originate from a single family of defects with a complex structure. Our results support this interpretation and indicate that

Spectral function and calculated photoluminescence spectrum

Figure 3. (a) Spectral function [S(ℏω)][S(\hbar\omega)] (black line, left axis) and partial Huang-Rhys factors (blue dots, right axis) with phonon energy, illustrating the energy-resolved electron-phonon coupling and dominant phonon modes associated with the a(2)→a(1)a(2) \rightarrow a(1) electronic transition in the C1hC_{1h}-PJT configuration of the NV−^{-} defect. (b) Calculated photoluminescence (PL) spectrum showing a pronounced ZPL emission at 1.80 eV and the vibronic sideband features, highlighting the role of electron-phonon coupling in the optical emission profile. The inset illustrates the dominant phonon mode at 87 meV.

the experimentally observed emission is consistent with nitrogen-vacancy-related centers in silicon nitride, rather than defects in a silica host [6]. Further controlled synthesis and targeted experiments will be essential to verify the microscopic origin of these single-photon emitters. Our findings will guide future efforts to isolate and engineer bright quantum emitters in silicon nitride.

In summary, we identify nitrogen-vacancy-related defects, particularly NV−^{-}, as the likely origin of the recently observed ∼2\sim2 eV single-photon emission in silicon nitride. The NV−^{-} exhibits a linearly polarized ZPL emission at 2.46 eV in the C1hC_{1h} configuration, with a lifetime of 9.01 ns and a high DW factor of 33%. We further show that pseudo-Jahn-Teller distortions generate symmetrically equivalent configurations (C1hC_{1h}-PJT), which modify the electronic structure and emission characteristics with a ZPL, lifetime, and DW factor of 1.80 eV, 10.17 ns, and 41%, respectively. The moderate electron-phonon coupling during the electronic transition gives a higher emission in the ZPL compared to the phonon-side band. Our study provides a microscopic understanding of bright quantum emitters and suggests that controlled creation of nitrogen-vacancy-related defects could enable deterministic integration of single-photon sources in silicon-nitride photonic circuits. This work lays the foundation for the design and implementation of scalable quantum photonic devices based on silicon nitride.

The authors thank the Materials Research Centre (MRC), the Supercomputer Education and Research Centre (SERC), and the Solid State and Structural Chemistry Unit (SSCU) at the Indian Institute of Science, Bangalore, for access to computing resources. This work was supported by the DST-Nanomission program of the Department of Science and Technology, Government of India (Grant No. DST/NM/TUE/QM-1/2019). S.M. acknowledges funding from the PMRF fellowship (ID No. 0201908). The authors also acknowledge support from the Institute of Eminence (IoE) scheme of the Ministry of Human Resource Development, Government of India.

Supplemental Materials: Origin of Bright Quantum Emissions with High Debye-Waller factor in Silicon Nitride

Bulk Properties

The bandgaps of β\beta-Si3_3N4_4 obtained from various theoretical approaches and experimental measurements are summarized in Table I. Our calculated bandgap using hybrid functional parameters AEXX = 0.3 and HFSCREEN = 0.2 closely matches both the G0W0G_0W_0 computed value and the experimentally reported bandgap of 6.5 eV for crystalline β\beta-Si3_3N4_4, as measured by linear fitting of EELS-STEM data by Asano et al. [11]. However, discrepancies persist among experimentally reported bandgap values in the literature.

MethodPBEDDHHSE06HSEa^{a}G0W0bG_0W_0^{b}Exp.c^{c}
EgE_g (eV)4.45.85.86.16.26.5

Table I. Bandgap of β\beta-Si3_3N4_4 obtained from various computational methods and experimental measurement.

a^{a}With AEXX=0.3 and HFSCREEN=0.2 b^{b}GW oneshot calculation c^{c}Experimental bandgap from linear fit in EELS-STEM [11]

Theoretical Methodology

Defect Formation Energy

The defect formation energy Ef[Xq]E^f[X^q] of a defect XX in charge state qq, as a function of the Fermi level EFE_F, is calculated using the expression [S2, S3]:

Ef[Xq]=Etot[Xq]−Etot[bulk]−∑iniμi+qEF+Ecorr(1)E^f[X^q] = E_{\mathrm{tot}}[X^q] - E_{\mathrm{tot}}[\mathrm{bulk}] - \sum_i n_i\mu_i + qE_F + E_{\mathrm{corr}} \tag*{(1)}

Here, Etot[Xq]E_{\mathrm{tot}}[X^q] and Etot[bulk]E_{\mathrm{tot}}[\mathrm{bulk}] are the total energies of the defect-containing and pristine bulk supercells, respectively. The term ∑iniμi\sum_i n_i\mu_i accounts for the exchange of atoms with reservoirs, where nin_i is the number of atoms of species ii added (ni>0n_i > 0) or removed (ni<0n_i < 0), and μi\mu_i is the corresponding chemical potential.

The chemical potentials are defined as follows:

  • Under N-rich conditions: μNN−rich=12Etot(N2)\mu_{\mathrm{N}}^{\mathrm{N-rich}} = \frac{1}{2}E_{\mathrm{tot}}(\mathrm{N}_2)

  • Under Si-rich conditions: μSiSi−rich=Etot(Si)\mu_{\mathrm{Si}}^{\mathrm{Si-rich}} = E_{\mathrm{tot}}(\mathrm{Si})

The remaining chemical potentials are derived from the constraint:

3μSi+4μN=μSi3N4(2)3\mu_{\mathrm{Si}} + 4\mu_{\mathrm{N}} = \mu_{\mathrm{Si_3N_4}} \tag*{(2)}

where μSi3N4\mu_{\mathrm{Si_3N_4}} is the total energy per formula unit of crystalline Si3_3N4_4.

The term qEFqE_F represents the energy required to exchange electrons with the reservoir defined by the Fermi level EFE_F. EcorrE_{\mathrm{corr}} includes finite-size corrections for potential alignment and charged defect interactions. We employ the extended Freysoldt-Neugebauer-Van de Walle (eFNV) correction as implemented in the DOPED package [13, 14].

Δ\DeltaSCF Calculation

For the C1h_{1h} configuration, the ground and excited states are both 2A′^2A' (doublets), while for the C1h_{1h}-PJT distorted structure (C1_1 symmetry), those are both 2A^2A. The ground and excited states of the C1h_{1h} configuration can be represented by single Slater determinants as

∣a′(1) a′(1)‾ a′(2)⟩and∣a′(1) a′(2)‾ a′(2)⟩,\left|a'(1)\,\overline{a'(1)}\,a'(2)\right\rangle\quad\text{and} \quad\left|a'(1)\,\overline{a'(2)}\,a'(2)\right\rangle,

respectively, where the overbar denotes electron occupation in the minority-spin channel.

Similarly, in the C1hC_{1h}-PJT configuration, the ground and excited states can be represented by single Slater determinants as

∣a(1) a(1)‾ a(2)⟩and∣a(1) a(2)‾ a(2)⟩,\left|a(1)\,\overline{a(1)}\,a(2)\right\rangle\quad\text{and} \quad\left|a(1)\,\overline{a(2)}\,a(2)\right\rangle,

respectively. Therefore, the Δ\DeltaSCF approach is applicable here because these correspond to doublet-to-doublet transitions dominated by single Slater determinants.

Photoluminescence and Electron-Phonon Coupling

To study the electron-phonon coupling and photoluminescence (PL) spectrum for defect-to-defect transitions, we use the theory of Huang and Rhys [38], as demonstrated by Alkauskas et al. [S6] and implemented in custom built DEFECTPL package [39]. The normalized PL lineshape is given by:

L(ℏω)=Cω3A(ℏω)(3)L(\hbar\omega) = C\omega^3 A(\hbar\omega) \tag*{(3)}

where the optical spectral function A(ℏω)A(\hbar\omega) is defined as:

A(ℏω)=∑m∣⟨χgm∣χe0⟩∣2δ(EZPL−Egm−ℏω)(4)A(\hbar\omega) = \sum_m \left|\langle\chi_{gm}|\chi_{e0}\rangle\right|^2 \delta(E_{ZPL} - E_{gm} - \hbar\omega) \tag*{(4)}

Here, χgm\chi_{gm} and χe0\chi_{e0} are vibrational wavefunctions of the ground and excited states, respectively, and Egm=∑knkℏωkE_{gm} = \sum_k n_k\hbar\omega_k is the energy of the ground-state vibrational level.

Assuming similar phonon modes in both states and using the generating function approach [40, 41], the spectral function becomes:

A(EZPL−ℏω)=12π∫−∞∞G(t)eiωt−γ∣t∣ dt(5)A(E_{ZPL} - \hbar\omega) = \frac{1}{2\pi}\int_{-\infty}^{\infty} G(t)e^{i\omega t-\gamma|t|}\,dt \tag*{(5)}

where G(t)=eS(t)−S(0)G(t) = e^{S(t)-S(0)} is the generating function and γ\gamma determines the ZPL width. The function S(t)S(t) is the Fourier transform of the electron-phonon coupling spectral function S(ℏω)S(\hbar\omega):

S(t)=∫0∞S(ℏω)e−iωt d(ℏω)(6)S(t) = \int_0^\infty S(\hbar\omega)e^{-i\omega t}\,d(\hbar\omega) \tag*{(6)}

The total Huang-Rhys factor is:

S(0)=∫0∞S(ℏω) d(ℏω)=∑kSk(7)S(0) = \int_0^\infty S(\hbar\omega)\,d(\hbar\omega) = \sum_k S_k \tag*{(7)}

Each partial HR factor SkS_k is given by:

Sk=ωkqk22ℏ(8)S_k = \frac{\omega_k q_k^2}{2\hbar} \tag*{(8)}

with:

qk=∑α,imα(Rα,i(e)−Rα,i(g))Δrk,α,i(9)q_k = \sum_{\alpha,i}\sqrt{m_\alpha}\left(R_{\alpha,i}^{(e)} - R_{\alpha,i}^{(g)}\right)\Delta r_{k,\alpha,i} \tag*{(9)}

Here, mαm_\alpha is the mass of atom α\alpha, Rα,i(g)R_{\alpha,i}^{(g)} and Rα,i(e)R_{\alpha,i}^{(e)} are atomic coordinates in the ground and excited states, and Δrk,α,i\Delta r_{k,\alpha,i} is the component of the normalized displacement vector of the kthk^{\text{th}} phonon mode.

The spectral function is then:

S(ℏω)=∑kSkδ(ℏω−ℏωk)(10)S(\hbar\omega) = \sum_k S_k\delta(\hbar\omega- \hbar\omega_k) \tag*{(10)}

The total HR factor S(0)S(0) quantifies the electron-phonon coupling and is reflected in the configuration coordinate change:

ΔQ=∑αmα(ΔRα)2(11)\Delta Q = \sqrt{\sum_\alpha m_\alpha(\Delta R_\alpha)^2} \tag*{(11)}

where ΔRα\Delta R_\alpha is the difference in atomic coordinates of atom α\alpha between ground and excited states.

Debye-Waller Factor and Localization Ratio

The Debye-Waller factor represents the fraction of emission in the ZPL, is:

wZPL=e−S(0)(12)w_{\mathrm{ZPL}} = e^{-S(0)} \tag*{(12)}

Phonon mode localization is estimated using the localization ratio:

βk=NIPRk(13)\beta_k = \frac{N}{IPR_k} \tag*{(13)}

where NN is the number of atoms in the supercell and IPRkIPR_k is the inverse participation ratio [S6]:

IPRk=1∑α(∑iΔrk,α,i2)2(14)IPR_k = \frac{1}{\sum_{\alpha}\left(\sum_i \Delta r_{k,\alpha,i}^{2}\right)^2} \tag*{(14)}

Radiative Transition Rate and Lifetime

The radiative transition rate Γrad\Gamma_{\mathrm{rad}} and lifetime τrad\tau_{\mathrm{rad}} are calculated as:

Γrad=1τrad=nrϵZPL3∣μˉ∣23πϵ0c3ℏ4(15)\Gamma_{\mathrm{rad}} = \frac{1}{\tau_{\mathrm{rad}}} = \frac{n_r\epsilon_{\mathrm{ZPL}}^3\lvert\bar{\mu}\rvert^2}{3\pi\epsilon_0c^3\hbar^4} \tag*{(15)}

Here, nr=2.0458n_r = 2.0458 is the refractive index of β\beta-Si3_3N4_4, and ∣μˉ∣\lvert\bar{\mu}\rvert is the magnitude of the transition dipole moment in eÅ. The constants ϵ0\epsilon_0, cc, and ℏ\hbar are used in units of e2eV⋅A˚\frac{\mathrm{e}^2}{\mathrm{eV}\cdot\text{\AA}}, Å/s, and eVs, respectively.

The transition dipole moment between ground and excited single-particle states is computed using the VaspBandUnfolding package [42]:

μk=iℏ(ϵf,k−ϵi,k)m⟨ψi,k∣p∣ψf,k⟩(16)\mu_k = \frac{i\hbar}{(\epsilon_{f,k}-\epsilon_{i,k})m}\langle\psi_{i,k}|\mathbf{p}|\psi_{f,k}\rangle \tag*{(16)}

Defect Thermodynamics in Si-Rich Conditions

Under Si-rich conditions, the nitrogen vacancy is found to be the most stable defect with a maximum formation energy reaching up to 4 eV for the neutral charge state. However, nitrogen substitution at silicon sites becomes energetically unfavorable with higher formation energies, resulting in less stable antisite and antisite-vacancy defects involving nitrogen.

ELECTRONIC STRUCTURE OF NEUTRAL NITROGEN VACANCY

Localization Ratio of Phonon Modes

Figure S3. Localization ratio of phonon modes for NV−NV^{-} defect in C1hC_{1h}-PJT configuration.

Migration Barrier

We performed nudged elastic band (NEB) calculation to evaluate the feasibility of a neighbouring nitrogen atom migrating from the nitrogen site adjacent to a silicon vacancy to the silicon vacancy site. As shown in Figure S4, our results indicate that this process involves a substantial energy barrier of 2.66 eV, as shown below. Furthermore, once the nitrogen atom is at the silicon site, the reverse transition back to the nitrogen site is also highly unlikely, with a calculated barrier of 2.04 eV.

Local Geometry

The bond lengths between atoms around NSiVN−N_{\mathrm{Si}}V_{\mathrm{N}}^{-} defect in the C1hC_{1h} configuration and the C1hC_{1h}-PJT configuration are shown in Figure S5.

Figure S5. Bond lengths (SiN, NN, and SiSi) around the NSiVNN_{\mathrm{Si}}V_{\mathrm{N}} defect in (a) the C1hC_{1h} configuration and (b) the C1hC_{1h}-PJT configuration. All bond lengths are given in angstrom (Å). The substituted nitrogen atom (shown in red) displaces by 0.37 Å during the distortion.

References

  1. [1]Aharonovich, I.; Englund, D.; Toth, M. Solid-state single-photon emitters. Nat. Photonics 2016, 10, 631641.DOI
  2. [2]Doherty, M. W.; Manson, N. B.; Delaney, P.; Jelezko, F.; Wrachtrup, J.; Hollenberg, L. C. The nitrogen-vacancy colour centre in diamond. Phys. Rep. 2013, 528, 1–45.DOI
  3. [3]Martin, Z. O.; Senichev, A.; Peana, S.; Lawrie, B. J.; Lagutchev, A. S.; Boltasseva, A.; Shalaev, V. M. Photophysics of Intrinsic Single-Photon Emitters in Silicon Nitride at Low Temperatures. Adv. Quantum Technol. 2023, 6, 2300099.arxiv.org/abs/2301.10809
  4. [4]Senichev, A.; Martin, Z. O.; Peana, S.; Sychev, D.; Xu, X.; Lagutchev, A. S.; Boltasseva, A.; Shalaev, V. M. Room-temperature single-photon emitters in silicon nitride. Sci. Adv. 2021, 7, eabj0627.
  5. [6]Chen, Y. C.; Lin, S. C.; Chou, J. P.; Tsai, Y. C.; Huang, C. T.; Lee, C. J.; Chang, W. H. Stable Single Photon Emitters with Large Debye–Waller Factor in Silica. ACS Photonics 2025, 12, 1461–1469.DOI
  6. [11]Asano, T.; Tezura, M.; Saitoh, M.; Tanaka, H.; Kikkawa, J.; Kimoto, K. Nanoscale observation of subgap excitations in β-Si₃N₄ with a high refractive index using low-voltage monochromated STEM: a new approach to analyze the physical properties of defects in dielectric materials. Appl. Phys. Express 2022, 15, 076501.DOI
  7. [13]Kumagai, Y.; Oba, F. Electrostatics-based finite-size corrections for first-principles point defect calculations. Phys. Rev. B 2014, 89, 195205.
  8. [14]Kavanagh, S. R.; Squires, A. G.; Nicolson, A.; Mosquera-Lois, I.; Ganose, A. M.; Zhu, B.; Brlec, K.; Walsh, A.; Scanlon, D. O. doped: Python toolkit for robust and repeatable charged defect supercell calculations. J. Open Source Softw. 2024, 9, 6433.DOI
  9. [16]Alkauskas, A.; Buckley, B. B.; Awschalom, D. D.; Van de Walle, C. G. First-principles theory of the luminescence lineshape for the triplet transition in diamond NV centres. New J. Phys. 2014, 16, 073026.DOI
  10. [21]Monkhorst, H. J.; Pack, J. D. Special points for Brillouin-zone integrations. Phys. Rev. B 1976, 13, 5188–5192.DOI
  11. [22]HARDIE, D.; JACK, K. H. Crystal Structures of Silicon Nitride. Nature 1957, 180, 323333.DOI
  12. [23]O’Hare, P.; Tomaszkiewicz, I.; Beck, II C.; Seifert, H.-J. Thermodynamics of silicon nitride. I. Standard molar enthalpies of formation ΔfHm at the temperature 298.15 K of α-Si₃N₄ and β-Si₃N₄. The Journal of Chemical Thermodynamics 1999, 31, 303–322.
  13. [24]Perdew, J. P.; Burke, K.; Ernzerhof, M. Generalized Gradient Approximation Made Simple. Phys. Rev. Lett. 1996, 77, 3865–3868.pubmed.ncbi.nlm.nih.gov/10062328
  14. [25]Gali, A.; Janzn, E.; Dek, P.; Kresse, G.; Kaxiras, E. Theory of Spin-Conserving Excitation of the N-V Center in Diamond. Phys. Rev. Lett. 2009, 103, 186404.DOI
  15. [26]Togo, A.; Tanaka, I. First principles phonon calculations in materials science. Scr. Mater. 2015, 108, 15.arxiv.org/abs/1506.08498
  16. [27]Dey, M.; Meher, S.; Singh, A. K. Carbon with Stone-Wales defect as quantum emitter in h-BN. Phys. Rev. B 2025, 111, 104109.DOI
  17. [28]Meher, S.; Dey, M.; Singh, A. K. High-throughput computational search for group-IV-related quantum defects as spin-photon interfaces in 4H-SiC. Phys. Rev. B 2025, 112, 184112.DOI
  18. [29]Grillo, M. E.; Elliott, S. D.; Freysoldt, C. Native defects in hexagonal β-Si₃N₄ studied using density functional theory calculations. Phys. Rev. B 2011, 83, 085208.DOI
  19. [30]Lenahan, P. M.; Curry, S. E. First observation of the ²⁹Si hyperfine spectra of silicon dangling bond centers in silicon nitride. Appl. Phys. Lett. 1990, 56, 157–159.DOI
  20. [31]Nantataki, F.; Shiraishi, K.; Iwata, J.-i.; Matsushita, Y.-i.; Oshiyama, A. Atomic and electronic structures of nitrogen vacancies in silicon nitride: Emergence of floating gap states. Phys. Rev. B 2022, 106, 155201.
  21. [32]Yuan, J.; Hou, Y.; Yang, Z.; Chen, F.; Li, Q. GaN as a Material Platform for Single Photon Emitters: Insights from Ab Initio Study. Adv. Opt. Mater. 2023, 11.DOI
  22. [33]Bersuker, I. The Jahn-Teller Effect; Cambridge University Press, 2006.DOI
  23. [34]Batalov, A.; Zierl, C.; Gaebel, T.; Neumann, P.; Chan, I.-Y.; Balasubramanian, G.; Hemmer, P. R.; Jelezko, F.; Wrachtrup, J. Temporal Coherence of Photons Emitted by Single Nitrogen-Vacancy Defect Centers in Diamond Using Optical Rabi-Oscillations. Phys. Rev. Lett. 2008, 100, 077401.pubmed.ncbi.nlm.nih.gov/18352594
  24. [35]Gali, A. Ab initio theory of the nitrogen-vacancy center in diamond. Nanophotonics 2019, 8, 19071943.DOI
  25. [36]Razinkovas, L.; Doherty, M. W.; Manson, N. B.; Van de Walle, C. G.; Alkauskas, A. Vibrational and vibronic structure of isolated point defects: The nitrogen-vacancy center in diamond. Phys. Rev. B 2021, 104, 045303.DOI
  26. [37]Maciaszek, M.; Žalandauskas, V.; Silkīnīs, R.; Alkauskas, A.; Razinkovas, L. The application of the SCAN density functional to color centers in diamond. J. Chem. Phys. 2023, 159.DOI
  27. [38]Huang, K.; A., R. Theory of light absorption and non-radiative transitions in F-centres. Proc. R. Soc. Lond. A 1950, 204, 406–423.
  28. [39]Meher, S.; Dey, M. DefectPl. 2024; https://github.com/Shibu778/defectpl, GitHub repository; accessed 15 May 2025.
  29. [40]Lax, M. The Franck-Condon Principle and Its Application to Crystals. J. Chem. Phys. 1952, 20, 1752–1760.DOI
  30. [41]Kubo, R.; Toyozawa, Y. Application of the Method of Generating Function to Radiative and Non-Radiative Transitions of a Trapped Electron in a Crystal. Prog. Theor. Phys. 1955, 13, 160–182.DOI
  31. [42]Zheng, Q. VaspBandUnfolding. 2023; https://github.com/QijingZheng/VaspBandUnfolding, GitHub repository; accessed 17 July 2023.

Paper details

vlnc:W_vtvwewzm
Version
v1 · latest
Published
Fresh — added to the Hub within the last 30 days
Added
License
CC BY 4.0
Usage

views · 0

downloads · 0

A view counts once per browser per day, a download each time the PDF is requested.

  • Physics and Astronomy

Not recorded for this paper

View statement
Looking for related papers…
Contents