betaFeedback

WorksPhysics and Astronomy

Effect of low-temperature compression on superconductivity and crystal structure in strontium metal

Abstract

The superconducting and structural properties of elemental strontium metal were investigated under pressures up to 60 GPa while maintaining cryogenic conditions during pressure application. Applying pressure at low temperatures reveals differences in superconducting and structural phases compared to previous reports obtained at room temperatures. Notably, the superconducting critical temperature exhibits a twofold increase under compression after cryogenic cooling within the pressure range of 35-42 GPa, compared to cryogenic cooling after room-temperature compression. Subsequently, the transition width becomes significantly sharper above 42 GPa. Low-temperature X-ray diffraction measurements under pressure reveal that this change corresponds to the Sr-III to Sr-IV transition, with no evidence of any metastable structure. Furthermore, the monoclinic Sr-IV structure was observed to remain stable to much higher pressures - at least up to 60 GPa, without the appearance of the incommensurate Sr-V phase present at room temperature. This implies that thermal activation energy plays an important role in overcoming the presence of a kinetic barrier to the Sr-V phase at room temperature.

Introduction

Pressure is a commonly used thermodynamic parameter to influence the structural properties of a material [1]. However, the structural modification can vary depending on the temperature at which pressure is applied [2]. This variation arises due to changes in the thermodynamic pathway leading to phase stability, which is closely related to both temperature and pressure. Applying pressure at low temperatures can lead to the formation of new metastable phases that are distinctly different from the structural trends observed at room temperatures [3]. Studies involving low-temperature pressurization below 140 K have identified a new barium phase, Ba-VI, which exhibits an orthorhombic structure (PnmaPnma) within a pressure range of 13 to 35 GPa [4]. The superconductivity in this Ba-VI phase was extensively investigated by Jackson et al. [5], revealing a maximum superconducting critical temperature (TcT_{\mathrm{c}}) near 8 K, which is twice that observed under high-pressure cooling, i.e. cryogenic cooling after room-temperature compression.

Among the alkaline earth elements, strontium (Sr) shares many similarities with barium (Ba), particularly in their complex structures. Notably, both elements exhibit intricate structures such as the incommensurate Sr-V [6] and Ba-IV phases [7, 8], comprised of two interpenetrating components (host and guest) that exhibit incommensurability along the cc-axis at room temperature. Previous structural studies under room-temperature compressions have identified several phases of strontium: Sr-I (fcc, Fm3ˉmFm\bar{3}m, 0-3.5 GPa) [9], Sr-II (bcc, Im3ˉmIm\bar{3}m, 3.5-26 GPa) [9], Sr-III (β\beta-tin, I41/amdI4_{1}/amd, 26-35 GPa) [10, 11], Sr-IV (monoclinic, IaIa, 35-46 GPa) [12], Sr-V (incommensurate, host-I4/mcmI4/mcm, guest-fct (face centered tetragonal), 46-74 GPa) [6]. Of particular interest is the Sr-IV phase, which exhibits a unique monoclinic structure characterized by a distortion of the tetragonal β\beta-tin Sr-III structure. This distortion results in a superstructure three times the size of the Sr-III unit cell, featuring a helical chain along the previous Sr-III cc-axis. This phenomenon is the result of rather small translations of atoms [13, 14].

Previous studies on the superconductivity of Sr have primarily been conducted under room-temperature compression followed by nearly isobaric cooling [15, 16, 17, 18]. Similar to Ba, the emergence of pressure-induced superconductivity in Sr is attributed to a significant s→ds \to d electron charge transfer with increasing pressure, supported by band structure calculations [18, 19, 20]. Interestingly, Sr exhibits a step-like increase in the Tc(P)T_{\mathrm{c}}(P) curve during the Sr-IV to Sr-V transition above 46 GPa during cryogenic cooling after room-temperature compression. Considering the discovery of the new metastable phase Ba-IV under low-temperature compression, which demonstrates a distinct TcT_{\mathrm{c}} compared to that observed under highpressure cooling, it is plausible that the same effect of low-temperature compression could lead to the formation of different crystal structures with unique superconducting properties in Sr. Despite extensive prior research, investigations into the superconducting and structural properties of Sr have largely focused on high-pressure applications at room temperature. In this study, we explore low-temperature compression paths to complement the past studies and gain deeper insights into the structural phases and superconductivity of elemental Sr metal.

Methods

For high-pressure electrical resistivity measurements, a 5N high-purity polycrystalline Sr sample was loaded into a membrane-driven diamond anvil cell (OmniDAC from Almax-easyLab) and placed inside a customized continuous-flow cryostat (Oxford Instruments) to facilitate in-situ pressure changes at low temperatures. A designer diamond anvil (with a 180 μ\mum culet size) equipped with tungsten leads was utilized [21]. Solid steatite (soapstone) served as the insulating and pressure-transmitting medium on the stainless steel gasket. Due to air sensitivity, the sample was loaded inside a nitrogen-filled glove box. The cell screws were then used to secure the sample and apply pressure (1 GPa). After attaching the membrane to the cell outside of the glove box, a small amount of helium gas pressure (∼\sim1 bar) was added to the membrane, and then the screws were removed. Subsequently, the membrane was employed to further increase the pressure. The sample was first pressurized at room temperature to 2 GPa and any subsequent increases in pressure were performed below 10 K. Pressure was determined using the fluorescence of the R1R_1 peak of small ruby chips [22] or the Raman signal of the anvil [23].

Resistance was measured in a four-probe arrangement using Keithly 6221 (DC current source) and Keithley 2182a (nanovoltmeter) configured for “delta mode.” The instruments were configured for resistance mode rather than voltage mode. In resistance mode, the instrument reports absolute values, such that when the signal becomes small, the noise appears with a floor at zero (see the inset to Figure 1). The electrical resistivity was estimated using the van der Pauw method, assuming isotropy in the sample plane: ρ=πtR/ln⁡2\rho= \pi t R/\ln2, where tt represents the sample thickness (∼\sim10 μ\mum). The resistivity is accurate to roughly a factor of two or three, considering uncertainties in the initial thickness of the sample. No adjustments were made for changes in sample thickness with pressure on the resistivity estimate. Further details of the nonhydrostatic high-pressure resistivity technique, including a photograph using a designer diamond anvil, are provided in Ref. [24].

Image not extracted

Figure 1. Temperature-dependent electrical resistivity of Sr under pressure up to 50 GPa, focusing on the superconducting transition. Pressure was applied below ∼\sim 10 K. Note that the transition becomes sharper above 42 GPa, potentially indicating a phase transition. Three downward arrows represent the criteria for the superconducting critical temperature (TcT_c) at 35 GPa with TcT_c(90%), TcT_c(50%), and TcT_c(10%), respectively (see text). The inset shows an expanded view of the zero-resistivity with a mean of ∼\sim20 nΩ\Omega-cm. This figure is adapted from Ref. [14].

High-pressure and low-temperature X-ray diffraction (XRD) measurements were conducted using two symmetric diamond anvil cells (DACs) with a diamond culet size of 300 μ\mum. This setup was housed in a cryostat equipped with a double membrane-driven pressurizing system at beamline 16-BM-D, Advanced Photon Source, Argonne National Laboratory. A 5N high-purity Sr sample was loaded into the DACs with a 140 μ\mum hole of pre-indented Re gasket (from 250 μ\mum down to 50 μ\mum) inside an argon-filled glove box with O2_2 levels below 0.5 ppm to prevent any oxidation, reaching initial pressures of 2-5 GPa without any pressure medium. X-ray beams with wavelengths of 0.4133 Å (30 keV) in Run 1 and 0.3100 Å (40 keV) in Run 2 were focused to a spot ∼\sim6×\times5 μ\mum2^2 (FWHM) in the sample with a tail of ∼\sim30×\times40 μ\mum2^2. The diffracted intensity was recorded using a Pilatus3 X CdTe 1M detector calibrated with a standard CeO2_2, with exposure times typically ranging from 60 to 120 seconds per image. Pressure was determined using the equation of state of Au grains loaded into the sample chamber, reflecting the temperature dependence within ranges of 15-296 K using Eq. (13) and Table 4 in Ref. [25]. DIOptAS [26] software converted 2D diffraction images to 1D diffraction patterns, subsequently analyzed by the Rietveld [27] or Le Bail [28] methods using the GSAS-II software [29]. Materials Project [30] was used to obtain the Crystallographic Information File (CIF) data and modify it for the different phases of the Sr sample, the Re gasket and the pressure marker Au.

Results

Figure 1 displays the temperature-dependent electrical resistivity data of Sr taken while loading pressure at low

temperatures below 10 K. The superconducting critical temperature (TcT_{\mathrm{c}}) is defined as TcT_{\mathrm{c}}(90%), TcT_{\mathrm{c}}(50%), and TcT_{\mathrm{c}}(10%) at which the resistivity has dropped to 90%, 50%, and 10% of the normal-state resistivity just above the transition. Superconductivity first appears at 35 GPa with a broad transition, with TcT_{\mathrm{c}}(50%) near 7 K as shown with a downward arrow. The superconducting transition width (ΔTc\Delta T_{\mathrm{c}}) is defined as the difference between TcT_{\mathrm{c}}(90%) and TcT_{\mathrm{c}}(10%), which is depicted as the upper and lower vertical bars in Figure 4(b). With increasing pressure, the transition temperature rises slowly accompanied by gradual increases in the normal-state resistivity, shown at 9.7 K at each pressure. When the pressure was increased to 42 GPa, it suddenly jumped to 48 GPa, although the resistivity in the normal state follows the same slope, increasing linearly with pressure. Interestingly, the superconducting transition suddenly becomes significantly sharper above 42 GPa to 50 GPa, the maximum pressure reached, with TcT_{\mathrm{c}}(90%) reaching 8.7 K (see the upper and lower vertical bars, ΔTc\Delta T_{\mathrm{c}}, of this work in Figure 4(b)). This abrupt change in ΔTc\Delta T_{\mathrm{c}} is reminiscent of the phase II to VI transition of Ba, an isoelectronic element of Sr, at low temperatures below 150 K [4], as there is a sharpening of the superconducting transition above 20 GPa across the structural transition [5]. It is not clear from the electrical resistivity data what may be happening in the pressure range across 42 GPa.

Image not extracted

Figure 4. Phase diagram of Sr focusing on (a) structural transitions and (b) corresponding superconductivity with the criterion Tc(50%)T_{\mathrm{c}}(50\%) (see text). Sr-IV at low temperatures (blue area) exhibits strong phase stability covering a wide pressure range. Closed symbols (or open symbols) in (a) refer to data with loading pressure (or unloading pressure). A white circle in (b) indicates that the pressure was extrapolated from the relationship between membrane pressure (bar) and sample pressure (GPa). Black downward arrows with bars refer to the lowest temperatures (5 K) found with no superconductivity at each pressure point. ρ\rho and χ\chi indicate electrical resistivity and magnetic susceptibility methods, respectively. The indications of the Sr structure at room temperature are shown at the top and bottom of (a) and (b), respectively, taken from Ref. [6, 9, 10, 11, 12]. The wide blue line in (b) corresponds to data taken with pressure applied at 10 K, while the wide grey line corresponds to data where pressure was applied at room temperature. This figure is modified from Ref. [14].

To investigate the abrupt change in the ΔTc\Delta T_{\mathrm{c}} above 42 GPa, we performed high-pressure and low-temperature XRD measurements on Sr, as illustrated in Figure 2. The 1D XRD patterns shown are from the measurements performed at the center of the sample. It is worth noting the presence of peak broadening with increasing pressure, indicating strain caused by non-hydrostatic pressure conditions. At room temperature, a structural transition from Sr-I (fcc, Fm3‾mFm\overline{3}m) to Sr-II (bcc, Im3‾mIm\overline{3}m) occurs 3.3 GPa in Run 2, depicted in Figure 2(b), consistent with previous studies [9]. After cooling to temperatures between 15 and 41 K, pressure was applied. Above 28 GPa at the low temperatures, Sr-II undergoes a transition to Sr-III (β\beta-tin, I41/amdI4_{1}/amd), slightly higher than the 26 GPa reported at room temperature [10, 11]. Sr-III persists up to 39 GPa, where it transforms to Sr-IV (monoclinic, IaI a). The transition pressure at room temperature was reported to be 35 GPa [12]. At low temperatures, Sr-IV remains stable up to 59.5 GPa, the highest pressure measured, in contrast to the phase transition from Sr-IV to Sr-V (incommensurate, host-I4/mcmI4/mcm, guest-fct) at 46 GPa at room temperature [6]. This highlights the strong stability of Sr-IV at low temperatures compared to room temperature, ruling out the potential presence of a metastable structure in Sr, unlike the metastable Ba-VI discovered only under low-temperature compression below the incommensurate structure of Ba-IV [4].

Image not extracted

Figure 2. Representative high-pressure XRD patterns of Sr under pressures up to 60 GPa at low temperatures between 15–41 K (except for 2.0 GPa and 3.3 GPa at room temperature), showing the structural transition (a) from Sr-II (bcc) through Sr-III (β\beta-tin) to Sr-IV (monoclinic) phases in Run 1 and (b) Sr-I (fcc) through Sr-II (bcc), Sr-III (β\beta-tin) to Sr-IV (monoclinic) in Run 2. The diffraction profiles from Sr-III and Sr-IV are similar as they only differ in slight distortion [13]. The small peak around 5.7 degrees at 2.0 GPa in Run 2 is unknown. A negligible second phase from Re (hcp) gasket or potentially oxidized SrO (fcc, Fm3‾mFm\overline{3}m) or possibly the S phase (previously reported as unknown) is present [11, 12, 31, 32].

The diffraction profiles of Sr-III and Sr-IV are similar, differing only in slight distortion [13].

Figure 3 shows representative Rietveld refinements of XRD patterns of Sr at five different pressures, displaying various phases from Runs 1 and 2, including Sr-I phase at room temperature and Sr-II, Sr-III, Sr-IV phases at low temperatures. The red and blue tick marks denote the expected locations of the Bragg peaks for the Re gasket [31] and Sr samples, respectively. A negligible second phase from the Re gasket (hcp, P63/mmcP6_{3}/mmc) [31] or SrO (fcc, Fm3‾mFm\overline{3}m) [32] is present. It is noteworthy that the room-temperature phase Sr-V (incommensurate, host-I4/mcmI4/mcm, guest-fct) [6] is absent, which significantly differs in diffraction profiles from Sr-IV (monoclinic, IaIa) [12]. All the refinements were carried out assuming preferred orientation of the crystalline grains using spherical harmonics since the raw detector images (see data repository [33]) show slightly irregular intensity over the Debye-Scherrer rings (slightly textured). All weighted profile RR factor (RwpR_{\mathrm{wp}}), which provides the goodness-of-fit (GOF) estimates, are below 5%. The XRD pattern at 2.0 GPa at room temperature is well-matched with the fcc Sr-I phase with the space group Fm3‾mFm\overline{3}m (Rwp=4.084%R_{\mathrm{wp}} = 4.084\%), in agreement with a previous study [9]. There is an unknown peak at around 5.7 degrees in 2θ2\theta, which is different from both SrO peaks and the 110 reflection (the first peak) from Sr-II arising in the phase boundary. The XRD pattern at 20.3 GPa and 24 K is well-refined with the bcc Sr-II phase with the space group Im3‾mIm\overline{3}m (Rwp=4.075%R_{\mathrm{wp}} = 4.075\%) [9]. The Sr-III phase is confirmed in the XRD pattern at 34.5 GPa and 23 K, which is the β\beta-tin (bct) structure with the space group I41/amdI4_{1}/amd (Rwp=4.010%R_{\mathrm{wp}} = 4.010\%) [10, 11]. At 43.8 GPa and 21 K, the diffraction pattern is refined with the monoclinic Sr-IV with the space group IaIa (Rwp=2.017%R_{\mathrm{wp}} = 2.017\%) [12]. The diffraction profiles of tetragonal β\beta-tin Sr-III and monoclinic Sr-IV are similar because they differ only in slight distortion resulting in a helical chain in the Sr-IV phase along the previous Sr-III cc-axis [13]. This phase persists to higher pressure at 55.9 GPa and 23 K (Rwp=3.5%R_{\mathrm{wp}} = 3.5\%) without undergoing the transition to the incommensurate Sr-V [6], which appears at room temperature.

Discussion

Figure 4 shows the phase diagrams of Sr illustrating (a) structural transitions and (b) corresponding superconductivity, which are modified from Ref. [14]. The structural phase diagram covering 0–300 K and 0–60 GPa in Figure 4(a) is constructed from the XRD data, as shown in Figure 2 and Figure 3. Run 1 (circle symbols) comprises 22 data points measured in the center of the sample and 24 data points measured in the position between the sample and the pressure marker Au near the edge of Re gasket. Run 2 (triangle symbols) has 19 data points measured in the center and 14 data points measured in the mixed position of the sample and Au located near the Re gasket. Black circles in Figure 4(b) represent the Tc(50%)T_{\mathrm{c}}(50\%) with loading pressure below 10 K. A white circle indicates that the pressure was extrapolated from the relationship between membrane pressure (bar) and sample pressure (GPa). The upper and lower vertical bars denote Tc(90%)T_{\mathrm{c}}(90\%) and Tc(10%)T_{\mathrm{c}}(10\%), respectively, indicating the transition width, ΔTc\Delta T_{\mathrm{c}}. The horizontal bars indicate the uncertainty of the pressure determination. The indications of the Sr structure at room temperature are shown at the top and bottom of (a) and (b), respectively, taken from Ref. [6, 9, 10, 11, 12]. The thick light blue and gray curves guide the eye for the data taken while compressing below 10 K and previous measurements where pressure was varied at room temperature [15, 16, 17], respectively.

Image not extracted

Figure 3. Representative Rietveld refinements of XRD patterns of Sr at five different pressures from Runs 1 and 2, depicting Sr-I (fcc, Fm3‾mFm\overline{3}m), Sr-II (bcc, Im3‾mIm\overline{3}m), Sr-III (β\beta-tin, I41/amdI4_{1}/amd), and Sr-IV (monoclinic, IaIa) phases. Note that the room-temperature phase Sr-V (incommensurate) is absent.

The phase boundaries depicted in Figure 4(a) shift towards higher pressures at low temperatures compared to room temperatures. The bcc Sr-II phase occupies a broad region of the structural phase diagram up to 28 GPa at low temperatures, where it transitions into the tetragonal β\beta-tin Sr-III phase. Notably, earlier theoretical studies [34, 35, 36] suggested that the Sr-III phase is energetically unfavorable relative to others. However, recent molecular dynamics (MD) and density functional theory (DFT) calculations by Tsuppayakorn-aek et al. [37] have accurately reproduced the experimental structure sequence using the screened exchange local density approximation (sX-LDA) functional, which treats dd electrons differently compared to other functionals. The upper boundary of the monoclinic Sr-IV phase in Figure 4(a) extends significantly to much higher pressures, at least up to 60 GPa, indicating its strong stability at low temperatures without transitioning to the incommensurate Sr-V structure present above 46 GPa at room temperatures. Ab initio random structure searching methods (AIRSS), coupled with density functional theory calculations by Kim et al. [36], reveal that the Sr-IV phase has a formation enthalpy comparable to the Sr-V phase above 35 GPa, with only a ∼\sim16 meV/atom difference at 50 GPa and zero temperature. The absence of the incommensurate Sr-V phase at low temperatures suggests that thermal activation energy might be crucial in overcoming the kinetic barrier between the Sr-IV and Sr-V phases at room temperature [38]. It is conceivable that low-temperature compression could mitigate the influence of unusually large anharmonic effects from the dd states near the Fermi level in Sr [14, 39], thereby reinforcing the strong phase stability of the monoclinic Sr-IV phase. The XRD measurements during unloading (depicted as open circle or triangle symbols) in Figure 4(a) demonstrate the reversibility of the structural phase boundaries.

Figure 4(b) illustrates the superconducting phase diagram of Sr, including samples compressed at low temperatures (Fig. 1 and those pressurized at room temperatures from previous studies [15, 16, 17]). A comparison to previously studied samples by Dunn et al. [15] and Bireckoven et al. [17] within the Sr-IV phase pressure range at room temperature reveals that Sr compressed at low temperatures exhibits a TcT_{\mathrm{c}} approximately twice as high. This observation could imply the presence of a structure different from Sr-IV when compressed at low temperatures, possibly indicating a metastable structure. However, the present XRD measurements find no additional structure at low-temperature compression to 60 GPa. Rather, they indicate that applying pressure at low temperatures stabilizes the Sr-III phase to a higher pressure, reaching 39 GPa, overlapping with the Sr-IV phase at room temperature, as depicted in Figure 4(a). This suggests that the Sr-III structure is being quenched to higher pressure at low temperatures, similar to the other phases. Notably, the Sr (III-IV) transition above 39 GPa at low temperatures aligns closely with the pressure where the change in the width ΔTc\Delta T_{\mathrm{c}} occurs above 42 GPa (within the small uncertainty of pressure determination). Additionally, a positive slope of dTc/dPdT_{\mathrm{c}}/dP in the Sr-III phase compressed at low temperature corresponds to that in the Sr-III phase compressed at room temperature.

The most recent electrical resistivity measurements by Mizobata et al. [16] closely align with the Tc(P)T_{\mathrm{c}}(P) dependencies observed in the present study, as depicted in Figure 4(b), due to similar experimental conditions. Both studies involved loading high-purity samples in a glove box and utilizing non-hydrostatic pressure environments in DACs. Minor variations in the Tc(P)T_{\mathrm{c}}(P) data likely arise from pressure gradients across the samples and shear stress induced by the non-hydrostatic pressure medium. It is widely recognized that such shear stresses can significantly influence Tc(P)T_{\mathrm{c}}(P) dependencies [40]. Note that some of the Tc(P)T_{\mathrm{c}}(P) data above 42 GPa, measured by Bireckoven et al. [17], agree with the present study, where it turns to the monoclinic Sr-IV at low temperatures. Kim et al. [36], employing AIRSS, DFT, electron-phonon coupling calculations, investigated the phase stability and superconductivity of Sr up to 50 GPa at 0 K. They identified an orthorhombic structure (CmcmCmcm) as stable above 25 GPa, exhibiting a TcT_{\mathrm{c}} of around 4 K within the pressure range of 30-55 GPa. This finding corresponds well the experimental TcT_{\mathrm{c}} measured by Dunn et al. [15] and Bireckoven et al. [17], as shown in Figure 4(b). However, the discrepancy in Tc(P)T_{\mathrm{c}}(P) data between low-temperature and room-temperature compression, particularly in the pressure range of 35-50 GPa, remains unclear and does not seem to stem from any potential metastable structure according to the current low-temperature XRD measurements. Dunn et al. [15] reported that the surface of the measured sample (99% purity) was oxidized, leading to a significant initial contact resistance. The presence of contamination could lead to sample homogeneity and suppress TcT_{\mathrm{c}} [41].

Conclusions

In summary, we conducted measurements on the superconducting and structural properties of elemental Sr metal up to 60 GPa under low-temperature compression. We observed a twofold increase in TcT_{\mathrm{c}} between 35-42 GPa compared to cryogenic cooling after room-temperature compression. Subsequently, the transition width became significantly sharper above 42 GPa. The results of low-temperature X-ray diffraction measurements under pressure indicate that this change corresponds to the Sr-III to Sr-IV transition, without the presence of any potential metastable structure similar to the high-pressure phase that was observed in cryogenic compression experiments on elemental Ba [5, 8]. Additionally, the monoclinic Sr-IV structure exhibited stability at significantly elevated pressures, reaching up to 60 GPa, without transitioning into the incommensurate Sr-V phase observed at room temperature. This suggests that thermal activation energy plays a crucial role in overcoming the kinetic barrier to the Sr-V phase at ambient temperature.

Data availability

All primary and analyzed data associated with the present study are publicly available via zenodo [33].

Acknowledgments

The development of high-pressure equipment and collection of electrical resistance data at the University of Florida was supported by the National Science Foundation CAREER award (DMR-1453752). Work at the University of Florida was performed under the auspices of the U.S. Department of Energy Basic Energy Sciences under Contract No. DE-SC-0020385 (xray data collection) and the U.S. National Science Foundation, Division of Materials Research under Contract No. NSF-DMR-2118718. We thank G. Fabbris (X-ray Science Division, Argonne National Laboratory) for his help in determining the pressure of the temperature-dependent equation of state of Au, and C. Kenney-Benson and R. Ferry for technical assistance (HPCAT). R.S.K. and R.J.H. acknowledge support from the U.S. National Science Foundation (DMR-2119308 and DMR-2104881). XRD measurements were performed at HPCAT (Sector 16), Advanced Photon Source (APS), Argonne National Laboratory. HPCAT operations are supported by the DOE-National Nuclear Security Administration (NNSA) Office of Experimental Sciences. The beamtime was made possible by the Chicago/DOE Alliance Center (CDAC), which is supported by DOE-NNSA (DE-NA0003975). The Advanced Photon Source is a DOE Office of Science User Facility operated for the DOE Office of Science by Argonne National Laboratory under Contract No. DE-AC02-06CH11357.

References

References

  1. [4]S. Desgreniers, J. S. Tse, T. Matsuoka, Y. Ohishi, Q. Li, and Y. Ma, Applied Physics Letters 107, 221908 (2015).
  2. [5]D. E. Jackson, D. VanGennep, Y. K. Vohra, S. T. Weir, and J. J. Hamlin, Phys. Rev. B 96, 184514 (2017).
  3. [6]M. I. McMahon, T. Bovornratanaraks, D. R. Allan, S. A. Belmonte, and R. J. Nelmes, Phys. Rev. B 61, 3135 (2000).
  4. [7]R. J. Nelmes, D. R. Allan, M. I. McMahon, and S. A. Belmonte, Phys. Rev. Lett. 83, 4081 (1999).
  5. [8]I. Loa, R. J. Nelmes, L. F. Lundegaard, and M. I. McMahon, Nature Materials 11, 627 (2012).
  6. [9]D. B. McWhan and A. Jayaraman, Applied Physics Letters 3, 129 (1963).
  7. [10]H. Olijnyk and W. Holzapfel, Physics Letters A 100, 191 (1984).
  8. [11]D. R. Allan, R. J. Nelmes, M. I. McMahon, S. A. Belmonte, and D. V. Bovornratanaraks, Rev. High Pressure Sci. Technol. 7, 236 (1998).
  9. [12]T. Bovornratanaraks, D. R. Allan, S. A. Belmonte, M. I. McMahon, and R. J. Nelmes, Phys. Rev. B 73, 144112 (2006).
  10. [13]H. Katzke and P. Toledano, Phys. Rev. B 75, 174103 (2007).
  11. [14]D. E. Jackson, Ph.D. thesis, University of Florida (2018).
  12. [15]K. J. Dunn and F. P. Bundy, Phys. Rev. B 25, 194 (1982).
  13. [16]S. Mizobata, T. Matsuoka, and K. Shimizu, Journal of the Physical Society of Japan 76, 23 (2007).
  14. [17]B. Bireckoven and J. Wittig, in Proc. 11 Int. Conf. AIRAPT, High Pressure Science and Technology, Vol. 3 (Naukova Dumka, 1989) pp. 14-24.
  15. [18]J. Hamlin, Physica C: Superconductivity and its Applications 514, 59 (2015).
  16. [19]H. L. Skriver, Phys. Rev. Lett. 49, 1768 (1982).
  17. [20]H. L. Skriver, Phys. Rev. B 31, 1909 (1985).
  18. [21]S. T. Weir, J. Akella, C. Aracne-Ruddle, Y. K. Vohra, and S. A. Catledge, Applied Physics Letters 77, 3400 (2000).
  19. [22]A. D. Chijioke, W. J. Nellis, A. Soldatov, and I. F. Silvera, Journal of Applied Physics 98, 114905 (2005).
  20. [23]Y. Akahama and H. Kawamura, Journal of Applied Physics 100, 043516 (2006).
  21. [24]J. Lim, A. C. Hire, Y. Quan, J. Kim, L. Fanfarillo, S. R. Xie, R. S. Kumar, C. Park, R. J. Hemley, Y. K. Vohra, R. G. Hennig, P. J. Hirschfeld, G. R. Stewart, and J. J. Hamlin, Phys. Rev. B 104, 064505 (2021).
  22. [25]W. B. Holzapfel, M. Hartwig, and W. Sievers, Journal of Physical and Chemical Reference Data 30, 515 (2001).
  23. [26]C. Prescher and V. B. Prakapenka, High Pressure Research 35, 223 (2015).
  24. [27]H. M. Rietveld, Journal of Applied Crystallography 2, 65 (1969).
  25. [28]A. Le Bail, H. Duroy, and J. Fourquet, Materials Research Bulletin 23, 447 (1988).
  26. [29]B. H. Toby and R. B. Von Dreele, Journal of Applied Crystallography 46, 544 (2013).
  27. [30]A. Jain, S. P. Ong, G. Hautier, W. Chen, W. D. Richards, S. Dacek, S. Cholia, D. Gunter, W. D. Skinner, G. Ceder, and K. A. Persson, APL Materials 1, 011002 (2013).
  28. [31]S. Anzellini, A. Dewaele, F. Occelli, P. Loubeyre, and M. Mezouar, Journal of Applied Physics 115, 043511 (2014).
  29. [32]L.-G. Liu and W. A. Bassett, Journal of Geophysical Research (1896-1977) 77, 4934 (1972).
  30. [33]All data associated with the present work are available online at https://zenodo.org/doi/10.5281/zenodo.11093188.
  31. [34]A. Pusittrakool, T. Bovornratanaraks, R. Ahuja, and U. Pinsook, Phys. Rev. B 77, 174118 (2008).
  32. [35]P. Srepusharawoot, W. Luo, T. Bovornratanaraks, R. Ahuja, and U. Pinsook, Solid State Communications 152, 1172 (2012).
  33. [36]D. Y. Kim, P. Srepusharawoot, C. J. Pickard, R. J. Needs, T. Bovornratanaraks, R. Ahuja, and U. Pinsook, Applied Physics Letters 101, 052604 (2012).
  34. [37]P. Tsuppayakorn-aek, W. Chaimayo, U. Pinsook, and T. Bovornratanaraks, AIP Advances 5, 097202 (2015).
  35. [38]J. Lim, J. S. Kim, A. C. Hire, Y. Quan, R. G. Hennig, P. J. Hirschfeld, J. J. Hamlin, G. R. Stewart, and B. Olinger, Journal of Physics: Condensed Matter 33, 285705 (2021).
  36. [39]N. Vaks, G. Samolyuk, and A. Trefilov, Physics Letters A 127, 37 (1988).
  37. [40]J. S. Schilling, High Pressure Research 26, 145 (2006).
  38. [41]J. Lim, S. Sinha, A. C. Hire, J. S. Kim, P. M. Dee, R. S. Kumar, D. Popov, R. J. Hemley, R. G. Hennig, P. J. Hirschfeld, G. R. Stewart, and J. J. Hamlin, Phys. Rev. B 108, 094501 (2023).

Paper details

vlnc:W_zxsru7e2
Version
v1 · latest
Published
Fresh — added to the Hub within the last 30 days
Added
License
CC BY 4.0
Usage

views · 0

downloads · 0

A view counts once per browser per day, a download each time the PDF is requested.

  • Physics and Astronomy

Not recorded for this paper

View statement
Looking for related papers…
Contents