betaFeedback

WorksPhysics and Astronomy

Electrical Stability of Cr2O3/\b{eta}-Ga2O3 and NiOx/\b{eta}-Ga2O3 Heterojunction Diodes

Abstract

This work reports the electrical characteristics comparison study between Cr2O3 and NiOx based heterojunction diodes (HJD) on halide vapor phase epitaxy (HVPE) grown \b{eta}-Ga2O3 epitaxial layers. Both as-fabricated Cr2O3 and NiOx HJDs exhibited forward current density in a range of 130-150 A/cm^2 at 5 V with rectifying ratios >10^10 and a reverse leakage current density at 10^-8 A/cm^2 at -5 V. The differential specific on-resistance of Cr2O3 and NiOx HJDs was 12.01 mΩcm^2 and 12.05 mΩcm^2, respectively. Breakdown voltages of Cr2O3 HJDs ranged from 1.4-1.9 kV and 1.5-2.3 kV for NiOx HJDs. Theoretical band alignment between Cr2O3 and \b{eta}-Ga2O3 was calculated from first principles. The ambient exposed NiOx/HVPE \b{eta}-Ga2O3 HJDs forward current density degraded after 10 days while that of Cr2O3/HVPE \b{eta}-Ga2O3 HJDs remained nearly unchanged after the same amount of time. It was later confirmed that the ambient exposed sputtered NiOx sheet resistance (Rsh) degradation gave rise to the reduction of the forward current density of the NiOx based HJDs, and water (H2O) was qualitatively determined to be the agent attributed to the forward conduction degradation by measuring the Rsh of NiOx-on-sapphire reference wafer after exposing it to different environments. The Cr2O3/HVPE \b{eta}-Ga2O3 HJD also exhibited enhanced thermal stability compared to the NiOx/\b{eta}-Ga2O3 heterostructures at elevated temperatures. Interfacial nickel gallate (Ga2NiO4) phase formation expected from phase diagrams can explain the reduced thermal stability of NiOx/\b{eta}-Ga2O3 HJDs. This study indicates that Cr2O3 is a stable p-type oxide for the realization of robust multi-kV \b{eta}-Ga2O3 HJDs.

Introduction

In recent years of wide/ultra-wide bandgap (WBG/UWBG) semiconductor advancements, β-Ga2O3\mathrm{Ga_2O_3} offers promising potential for medium-voltage power applications (1-35 kV) in applications of grid transmission, renewable energy processing, and data centers for artificial intelligence (AI). The high critical electric field strength and availability of the shallow hydrogenic dopants[1] in epitaxial β-Ga2O3\mathrm{Ga_2O_3}[2, 3, 4, 5] can be leveraged to demonstrate power devices with much lower differential specific on-resistance while operating at a higher blocking voltage[6, 7, 8] compared to silicon carbide (SiC) and gallium nitride (GaN)[9, 10]. Although reliable p-type doping with mobile holes in β-Ga2O3\mathrm{Ga_2O_3} is currently unavailable, p-type oxides, such as nickel oxide (NiO), have been integrated with β-Ga2O3\mathrm{Ga_2O_3} to form P-N heterojunctions that readily enable multi-kV junctions[11, 12, 13, 14, 15, 16] with breakdown voltage >10>10 kV[17, 18, 19] and high electric field at 7.5 MV/cm2\mathrm{cm^2}[20]. Several materials issues in NiO/β\beta-Ga2_2O3_3 heterojunction-based power devices. For example, instability of sputtered NiO under ambient exposure results in fluctuation of acceptor concentration (NAN_\mathrm{A}) in this material, requiring a 15-minute nitrogen (N2\mathrm{N}_2) anneal at 275 °C for stabilization[19, 21, 22, 23, 24]. Recently, it was also reported that the NiO/β\beta-Ga2_2O3_3 heterojunction interface is susceptible to secondary nickel gallate (Ga2_2NiO4_4) phase formation[25, 26], which affects the thermal stability of the junction characteristics. Stable p-type oxide/β\beta-Ga2_2O3_3 heterojunction diodes with no interfacial phase formation are therefore necessary for reliable applications in β\beta-Ga2_2O3_3-based power electronics.

Chromium oxide (Cr2_2O3_3), a p-type oxide[27] with a bandgap of ~3.6 eV[28, 29], has recently been explored to form P-N heterojunctions[30, 31, 32] with β\beta-Ga2_2O3_3 as an alternative to NiO-based junctions, exhibiting enhanced thermal stability under high temperature environment at 600 °C[32].

In this work, we compared the electrical characteristics of as-fabricated Cr2_2O3_3/HVPE β\beta-Ga2_2O3_3 and NiOx_x/HVPE β\beta-Ga2_2O3_3 HJDs. Theoretical band alignment between Cr2_2O3_3 and β\beta-Ga2_2O3_3 is reported by first-principles calculations. Forward current density of HJDs and oxide sheet resistance variation under ambient exposure were also tracked to compare the material stability. Water vapor (H2_2O) in the air was qualitatively found to be the cause for degradation of the sheet resistance in sputtered NiOx_x exposed to ambient conditions. Temperature-dependent J-V measurements confirmed the enhanced thermal stability of Cr2_2O3_3-based HJDs at elevated temperatures. The enhanced thermal stability of Cr2_2O3_3/β\beta-Ga2_2O3_3 interface is further corroborated from the absence of a stable ternary phase in the Cr-Ga-O system compared to the Ga2_2NiO4_4 phase formation at the NiO/β\beta-Ga2_2O3_3 heterojunction interface by comparing their theoretical phase diagrams.

Device Fabrication

The Cr2_2O3_3/HVPE β\beta-Ga2_2O3_3 heterojunction diode (HJD) fabrication began with a backside Ti/Au (50/150 nm) Ohmic metallization on n+^+ β\beta-Ga2_2O3_3 bulk substrate using e-beam evaporation followed by a 60-seconds rapid thermal annealing (RTA) at 470 °C in N2\mathrm{N}_2. Following the backside Ohmic contact formation, a photoresist lift-off mask was patterned using optical lithography after standard solvent clean (acetone/isopropanol/de-ionized water). Then, a ~20-nm p−^- Cr2_2O3_3 layer (Rsheet_\mathrm{sheet} ~1 MΩ\Omega/□) was directly deposited on the HVPE β\beta-Ga2_2O3_3 via reactive radio frequency (RF) magnetron sputtering by using a 99.95%-pure metallic chromium (Cr) target under an oxygen-deficient condition (Ar/O2_2~22/10 sccm) at a 3.7 mTorr chamber pressure and 150 W RF power. To enhance the Ohmic contact quality to Cr2_2O3_3, a ~20-nm p+^+ Cr2_2O3_3 contact layer (Rsheet_\mathrm{sheet}~600 kΩ\Omega/□) was sputtered under an oxygen-rich condition (Ar/O2_2~8/10 sccm) at a 3 mTorr chamber pressure and the same RF power. The atomic percentage of Cr (30.6%) and O (69.4%) were confirmed by using energy dispersive spectroscopy (EDS) on reference silicon monitor wafer, closely matching the stoichiometry of Cr2_2O3_3 reported[30] earlier. Immediately following the sputter deposition, a Ni/Au/Ni\mathrm{Ni}/\mathrm{Au}/\mathrm{Ni} (50/50/200 nm) metal stack was deposited via e-beam evaporation to serve as an Ohmic contact to Cr2O3\mathrm{Cr}_{2}\mathrm{O}_{3} and a hard mask for subsequent plasma dry etching[20, 33]. The Cr2O3\mathrm{Cr}_{2}\mathrm{O}_{3}/Ohmic metal stack was later lifted off in a heated N-methyl pyrrolidone (NMP) solution. To mitigate the electric field crowding, the diodes were dry-etched ∼1.2\sim1.2 μ\mum below the Cr2O3\mathrm{Cr}_{2}\mathrm{O}_{3}/β\beta-Ga2O3\mathrm{Ga}_{2}\mathrm{O}_{3} heterojunction interface under inductively coupled BCl3\mathrm{BCl}_{3} plasma at 200 W, as shown in Figure 1(a). This self-aligned plasma-etch served as edge termination for the device. Similarly, the NiOx\mathrm{NiO}_{x}/HVPE β\beta-Ga2O3\mathrm{Ga}_{2}\mathrm{O}_{3} HJDs, as shown in Figure 1(b), were also fabricated on the same wafer by using a sputtering condition of Ar/O2∼22/10_{2}\sim22/10 sccm at a 3.7 mTorr chamber pressure and 150 W RF power for ∼\sim20-nm of p−^{-} NiOx\mathrm{NiO}_{x} (Rsheet∼215R_{\mathrm{sheet}}\sim215 kΩ\Omega/□) and Ar/O2∼8/10_{2}\sim8/10 sccm at a 3 mTorr chamber pressure and 150 W RF power for ∼\sim20-nm of p+^{+} NiOx\mathrm{NiO}_{x} (Rsheet∼7R_{\mathrm{sheet}}\sim7–9 kΩ\Omega/□) by using the identical fabrication process[20, 33]. The NiOx\mathrm{NiO}_{x} layers were sputtered from a 99.999% purity nickel (Ni) metallic target.

Figure 1. (a) Cr2O3\mathrm{Cr}_{2}\mathrm{O}_{3}/HVPE β\beta-Ga2O3\mathrm{Ga}_{2}\mathrm{O}_{3} heterojunction diode with ∼1.2\sim1.2 μ\mum plasma-etch edge termination schematics. (b) NiOx\mathrm{NiO}_{x}/HVPE β\beta-Ga2O3\mathrm{Ga}_{2}\mathrm{O}_{3} heterojunction diode with ∼1.2\sim1.2 μ\mum plasma-etch edge termination schematics.

Cr2O3\mathrm{Cr}_{2}\mathrm{O}_{3}/β\beta-Ga2O3\mathrm{Ga}_{2}\mathrm{O}_{3} Band Alignment Calculation

We use the electronic transition level of hydrogen to align the band structures.[34] We perform first-principles calculations to locate the (+/−) transition level of interstitial hydrogen in β\beta-Ga2O3\mathrm{Ga}_{2}\mathrm{O}_{3} and corundum Cr2O3\mathrm{Cr}_{2}\mathrm{O}_{3}. Our calculations are based on the generalized Kohn-Sham theory[35] using the HSE hybrid functional[36] implemented with projector augmented wave (PAW) potentials[37, 38] in the VASP code.[39] In the HSE functional, the mixing parameters are fitted to reproduce experimental band gaps and lattice constants: 34% for β\beta-Ga2O3\mathrm{Ga}_{2}\mathrm{O}_{3} and 18% for corundum Cr2O3\mathrm{Cr}_{2}\mathrm{O}_{3}. With these parameters, we obtain for β\beta-Ga2O3\mathrm{Ga}_{2}\mathrm{O}_{3} an indirect band gap of 4.81 eV and lattice parameters a=a = 12.2512.25 Å, b=3.04b = 3.04 Å and c=5.81c = 5.81 Å. For corundum Cr2_2O3_3 we obtain an indirect band gap of 3.45 eV and lattice parameters a=4.97a = 4.97 Å and c=13.65c = 13.65 Å.

We employed 120-atom supercells; for β\beta-Ga2_2O3_3 this corresponds to a 1×3×21 \times3 \times2 multiple of the 20-atom monoclinic conventional cell, and for corundum Cr2_2O3_3 to a 2×2×12 \times2 \times1 multiple of the 30-atom hexagonal conventional cell. Calculations are performed using a 2×2×22 \times2 \times2 k-point grid and a plane-wave cutoff energy of 500 eV. Spin polarization is included. For an interstitial hydrogen impurity in charge state qq (±1\pm1), the formation energy is given by40

Ef(Hiq)=Et(Hiq)−Et(bulk)−μH+qEF+Δq,(1)E^{f}(\mathrm{H}_{\mathrm{i}}^{q}) = E_{\mathrm{t}}(\mathrm{H}_{\mathrm{i}}^{q}) - E_{\mathrm{t}}(\mathrm{bulk}) - \mu_{\mathrm{H}} + qE_{\mathrm{F}} + \Delta^{q}, \tag*{(1)}

where Ef(Hiq)E^{f}(\mathrm{H}_{\mathrm{i}}^{q}) is the formation energy of the interstitial hydrogen in charge state qq, Et(Hiq)E_{\mathrm{t}}(\mathrm{H}_{\mathrm{i}}^{q}) and Et(bulk)E_{\mathrm{t}}(\mathrm{bulk}) are the total energies of the defective and pristine supercells, and μH\mu_{\mathrm{H}} is the chemical potential of hydrogen. The term qEFqE_{\mathrm{F}} accounts for the exchange of electrons with the reservoir, where the Fermi level EFE_{\mathrm{F}} is referenced to the VBM. Δq\Delta^{q} represents the finite-size correction for charged supercells, following established schemes.41,42

Due to the monoclinic crystal structure of β\beta-Ga2_2O3_3, multiple configurations are possible for Hi+_{\mathrm{i}}^{+} and Hi−_{\mathrm{i}}^{-}. In the lowest energy structures, Hi+_{\mathrm{i}}^{+} bonds to a lone pair of three-fold coordinated oxygen atom whereas Hi−_{\mathrm{i}}^{-} relaxes to a site near two Ga atoms within the mirror plane perpendicular to the bb axis. These configurations yield a (+/−) transition level 0.04 eV above the CBM as shown in Figure 2, in agreement with previous work.43 In corundum Cr2_2O3_3, both Hi+_{\mathrm{i}}^{+} and Hi−_{\mathrm{i}}^{-} bond to a four-fold coordinated oxygen atom. In the donor state (Hi+_{\mathrm{i}}^{+}), the four Cr-O bonds elongate by 3%, 4%, 6% and 10%. In the acceptor state Hi−_{\mathrm{i}}^{-}, three Cr-O bonds elongate by 0.5%, 15%, 20% while the fourth shortens by 1%. The resulting (+/−) level is located 0.44 eV below the CBM. In Figure 2, we align the transition level (+/-) of interstitial hydrogen in β\beta-Ga2_2O3_3 and corundum Cr2_2O3_3, resulting in a type-II band alignment for the heterojunction, with valence- and conduction-band offsets of ΔEv=1.85\Delta E_{\mathrm{v}}=1.85 eV and ΔEc=0.48\Delta E_{\mathrm{c}}=0.48 eV.

Band alignment between $\beta$-Ga$_2$O$_3$ and corundum Cr$_2$O$_3$

Figure 2. Band alignment between β\beta-Ga2_2O3_3 and corundum Cr2_2O3_3. The valence bands are shown in red and the conduction bands in blue. The dashed line indicates the (+/−) transition level of interstitial hydrogen.

β\beta-Ga2_2O3_3 HJDs Electrical Characteristics Analysis

High-Voltage Capacitance-Voltage (C-V) Analysis

The punch-through electric field profile of Cr2_2O3_3/β\beta-Ga2_2O3_3 HJDs beyond ∼600\sim600 V was confirmed via high-voltage capacitance–voltage measurements at 1 MHz, as shown in Figure 3(a). The HVPE layer was fully depleted above 600 V reverse bias, where measured capacitance remained flat and no longer changed as a function of applied reverse bias. Moreover, the built-in potential (VbiV_{\mathrm{bi}}) of the HVPE HJD was extracted to be ∼2\sim2 V from the 1/C21/C^2 vs voltage characteristics shown in Figure 3(a) inset, closely matching the VbiV_{\mathrm{bi}} extracted from NiOx_x/β\beta-Ga2_2O3_3 HJDs from our early reports[20, 33]. The average HVPE drift layer's apparent charge density was extracted to be 9.5×10159.5 \times10^{15} cm−3^{-3} with a corresponding thickness of ∼7.48\sim7.48 μ\mum using a relative permittivity of 12.4[44] for (001) β\beta-Ga2_2O3_3, as shown in Figure 3(b).

High-voltage C–V characteristics and extracted apparent charge density profile

Figure 3. (a) High-voltage C–V characteristics on 1-mm2^{2} area pad at 1 MHz with inset showing the built-in potential of Cr2_{2}O3_{3}/HVPE β-Ga2_{2}O3_{3} HJD. (b) Extracted apparent charge density vs depth profile of the plasma-etched Cr2_{2}O3_{3}/HVPE β-Ga2_{2}O3_{3} vertical HJD.

J-V & Reverse Breakdown Characteristics

The forward linear J-V characteristics of the Cr2_{2}O3_{3}/HVPE β-Ga2_{2}O3_{3} and NiOx_x/HVPE β-Ga2_{2}O3_{3} HJDs on 100-μm dia. devices are shown in Figure 4(a) by considering a 45°-angle current spreading[33, 45]. Both types of HJDs exhibit comparable on-state current density in a range of 130–150 A/cm2^{2} at 5 V. The rectifying ratio of both types of HJDs are >1010^{10} with a reverse leakage of ~10−8^{-8} A/cm2^{2} at -5 V and ideality factors of 1.72 and 1.63 for Cr2_{2}O3_{3} and NiOx_x HJDs, respectively, as shown in Figure 4(b). The minimum differential specific on-resistance of the Cr2_{2}O3_{3} and NiOx_x-based HJDs are extracted to be 12.01 mΩ•cm2^{2} and 12.05 mΩ•cm2^{2}, respectively, as shown in Figure 4(c). The reverse leakage and breakdown characteristics of the HJDs (submerged in FC-40 Fluorinert liquid) on HVPE β-Ga2_{2}O3_{3} for 100-μm dia. devices are shown in Figure 4(d), showing a breakdown voltage range of 1.4–1.9 kV for Cr2_{2}O3_{3}/β-Ga2_{2}O3_{3} HJDs and 1.5–2.3 kV for NiOx_x/β-Ga2_{2}O3_{3} HJDs with noise-floor reverse leakage current densities (10−8^{-8}~10−6^{-6} A/cm2^{2}, nA) at 80% of the devices’ catastrophic breakdown voltage for both types of HJDs.

Four-panel J-V and reverse breakdown characteristics of Cr₂O₃/β-Ga₂O₃ and NiOₓ/HVPE β-Ga₂O₃ HJDs

Figure 4. (a) Linear J-V characteristics of Cr₂O₃/β-Ga₂O₃ and NiOₓ/HVPE β-Ga₂O₃ HJDs on 100-μm dia. device with a 45°-angle current spreading effect. (b) Semi-log scale J-V characteristics of Cr₂O₃/β-Ga₂O₃ and NiOₓ/HVPE β-Ga₂O₃ HJD on 100-μm dia. device with a 45°-angle current spreading effect. (c) Ron,spR_{\mathrm{on,sp}} vs. voltage of Cr₂O₃/β-Ga₂O₃ and NiOₓ/HVPE β-Ga₂O₃ HJDs on 100-μm dia. device with a 45°-angle current spreading effect. (d) Reverse breakdown characteristics of Cr₂O₃/β-Ga₂O₃ and NiOₓ/HVPE β-Ga₂O₃ HJD on 100-μm dia. devices.

Electrical Stability under Ambient Conditions & Elevated Temperatures

The J-V characteristics of both as-fabricated Cr₂O₃/β-Ga₂O₃ and NiOₓ/HVPE β-Ga₂O₃ HJDs were tracked as deposited, after 3 days, and after 10 days by exposing samples to the ambient. It was observed that the as-deposited current density of Cr₂O₃ HJD exhibited comparable value with that of NiOₓ HJD at 4 V, as shown in Figure 5(a). After 3 days of ambient exposure, the Cr₂O₃ HJD current density decreased slightly in the vicinity of 120 A/cm² at 4 V similar to what it was as deposited, but the NiOₓ HJD current density significantly dropped below 15 A/cm². After 10 days of ambient exposure, the Cr₂O₃ HJD remained around 120 A/cm² at 4 V while the NiOₓ HJD current density continued to decrease to < 1 A/cm², indicating electrical instability of NiOₓ/HVPE β-Ga₂O₃ HJDs. To identify the cause of this degradation of the HJD’s on-state degradation, Cr₂O₃ and NiOₓ layers were sputtered on sapphire with Ni/Au Ohmic contact for four-point Van Der Pauw measurements. It was observed that the sheet resistance (RshR_{\mathrm{sh}}) of the sputtered NiOₓ on sapphire gradually increased to 50% of its original RshR_{\mathrm{sh}} value within 21 days, as shown in Figure 5(b) while the RshR_{\mathrm{sh}} of Cr₂O₃ varied less than 10% of its original RshR_{\mathrm{sh}} value, implying enhanced electrical stability of Cr₂O₃ under ambient exposure compared to NiOₓ. To further investigate the origin of the sheet resistance degradation in sputtered NiOₓ degradation, the NiOₓ on sapphire was exposed to different environments, and the sheet resistance variation was tracked after 72 hours exposure, as shown in Figure 5(c). A metal-organic chemical vapor deposition (MOCVD) reactor with high purity oxygen (O₂, 500 Torr) and nitrogen gas (N₂, 500 Torr) flow was used to expose the sample to N₂ and O₂. It was observed that the RshR_{\mathrm{sh}} of sputtered NiOₓ varied insignificantly within 72 hours when it was placed in pure N₂ and O₂, and the variation was comparable to the case where the reference sputtered NiOₓ on sapphire was sealed in vacuum post deposition. Upon submerging the NiOₓ-on-sapphire sample in de-ionized water (H₂O), the RshR_{\mathrm{sh}} degraded ~10% within 72 hours, which was similar to the extent of degradation when the NiOx_x/Al2_2O3_3 was exposed in ambient for the same amount of time. Therefore, it was qualitatively concluded that H2_2O is the agent that potentially causes the degradation in sputtered NiOx_x.

Linear J-V characteristics, sheet resistance variation over time, and sheet resistance variation under exposure conditions

Figure 5. (a) Linear J-V characteristics of Cr2_2O3_3/β-Ga2_2O3_3 and NiOx_x/HVPE β-Ga2_2O3_3 HJDs tracked as deposited, after 3-day, and after 10-day. (b). Sheet resistance variation of sputtered Cr2_2O3_3 and NiOx_x on reference sapphire wafers within 30-day. (c) Sheet resistance variation of sputtered NiOx_x under various exposure conditions within 72 hours.

Beyond J-V characterization of ambient exposed Cr2_2O3_3 HJDs, temperature-dependent J-V characteristics of the HJDs were measured to examine the diodes’ thermal stability under elevated temperatures from 25 °C to 175 °C, as shown in Figure 6(a).

Temperature-dependent J-V characteristics and on-resistance temperature power law fit

Figure 6. (a) Temperature-dependent J-V characteristics of Cr2_2O3_3/HVPE β-Ga2_2O3_3 HJDs from 25 °C to 175 °C in semi-log scale (left) and linear scale (right). (b) Cr2_2O3_3/HVPE β-Ga2_2O3_3 HJDs on-resistance vs. temperature power law fit.

The temperature-resistance dependent coefficient (α) was extracted from the power law fit of the on-resistance of the HJD as a function of temperatures, as shown in Figure 6(b). The extracted α of the Cr2_2O3_3/HVPE β-Ga2_2O3_3 HJD was lower than that of NiOx_x/HVPE β-Ga2_2O3_3 HJD (α=1.56)[33] from previous literatures, indicating thermal stability[32] of sputtered Cr2_2O3_3 relative to NiOx_x. Since the temperature-dependent sweep was carried out 10 days after the diode’s ambient exposure, the NiOx_x/HVPE β\beta-Ga2_2O3_3 HJDs’ on-state characteristics were heavily degraded, and no consistent variation trend was observed.

Ternary (Ga-Ni-O, Ga-Cr-O) Compositional Phase Diagram

To further investigate the thermal instability in NiOx_x/β\beta-Ga2_2O3_3 heterojunction, the ternary compositional phase diagram of Ga-Ni-O and Ga-Cr-O systems generated by The Materials Project[46] database are compared in Figure 7(a) and Figure 7(b), respectively, to examine any interfacial reaction hindering thermal stability of HJDs.

Figure 7. (a) Ternary phase diagram of Ga-Ni-O system. (b) Ternary phase diagram of Ga-Cr-O system.

Experimental observation of nickel gallate (Ga2_2NiO4_4)[25, 26] for the NiOx_x/β\beta-Ga2_2O3_3 heterostructure system matches well with the stable phase predicted from the phase diagram. For the Ga-Cr-O system, there is no predicted stable intermediate phase formation at the Cr2_2O3_3/β\beta-Ga2_2O3_3 heterojunction, indicating enhanced material system stability.

Conclusion

In summary, this work explored the comparison of electrical performances of NiOx_x/HVPE β\beta-Ga2_2O3_3 and Cr2_2O3_3/HVPE β\beta-Ga2_2O3_3 heterojunction diodes. It was discovered that the as-deposited NiOx_x and Cr2_2O3_3 HJDs exhibited similar electrical characteristics in terms reverse leakage current density, differential specific on-resistance, and breakdown voltages. A type-II band alignment between Cr2_2O3_3 and β\beta-Ga2_2O3_3 was determined from first-principles calculations. The NiOx_x HJDs’ forward conduction gradually degraded over extended period while the Cr2_2O3_3 HJDs’ forward conduction remained nearly constant, and H2_2O is qualitatively identified as the agent that caused sheet resistance degradation in ambient exposed sputtered NiOx\mathrm{NiO}_{x}. Temperature dependent J-V characteristics also revealed thermal stability in Cr2O3\mathrm{Cr}_{2}\mathrm{O}_{3}/HVPE β\beta-Ga2O3\mathrm{Ga}_{2}\mathrm{O}_{3} heterostructures relative to as-fabricated Cr2O3\mathrm{Cr}_{2}\mathrm{O}_{3}/HVPE β\beta-Ga2O3\mathrm{Ga}_{2}\mathrm{O}_{3} HJDs.

Acknowledgments

The authors acknowledge funding from the U.S. Department of Energy (DOE) ARPA-E ULTRAFAST program (DE-AR0001824) and Coherent/II-VI Foundation Block Gift Program, and SUPREME, one of seven centers in JUMP 2.0, a Semiconductor Research Corporation program sponsored by the Defense Advanced Research Projects Agency. This research also used resources of the National Energy Research Scientific Computing Center, a DOE Office of Science User Facility supported by the Office of Science of the U.S. Department of Energy under Contract No. DE-AC02-05CH11231 using NERSC Award No. BES-ERCAP0028497. A portion of this work was performed at the UCSB Nanofabrication Facility, an open access laboratory.

Data Availability

The data that supports the findings of this study are available from the corresponding authors upon reasonable request.

References

  1. [1]1 A.T. Neal, S. Mou, S. Rafique, H. Zhao, E. Ahmadi, J.S. Speck, K.T. Stevens, J.D. Blevins, D.B. Thomson, and N. Moser, “Donors and deep acceptors in β-Ga₂O₃,” Applied Physics Letters 113(6), (2018).DOI
  2. [2]2 A. Bhattacharyya, C. Peterson, K. Chanchaiworawit, S. Roy, Y. Liu, S. Rebollo, and S. Krishnamoorthy, “Over 6 μm thick MOCVD-grown low-background carrier density (10¹⁵ cm⁻³) high-mobility (010) β-Ga₂O₃ drift layers,” Applied Physics Letters 124(1), (2024).DOI
  3. [3]3 C. Peterson, A. Bhattacharyya, K. Chanchaiworawit, R. Kahler, S. Roy, Y. Liu, S. Rebollo, A. Kallistova, T.E. Mates, and S. Krishnamoorthy, “200 cm²/Vs electron mobility and controlled low 1015 cm - 3 Si doping in (010) β-Ga₂O₃ epitaxial drift layers,” Applied Physics Letters 125(18), (2024).
  4. [4]4 S. Rebollo, Y. Liu, C. Peterson, S. Krishnamoorthy, and J.S. Speck, “Growth of nitrogen-doped (010) β-Ga₂O₃ by plasma-assisted molecular beam epitaxy using an O₂/N₂ gas mixture,” Applied Physics Letters 126(8), (2025).DOI
  5. [5]5 C. Peterson, C.N. Saha, R. Kahler, Y. Liu, A. Mattapalli, S. Roy, and S. Krishnamoorthy, “Kilovolt-class β-Ga₂O₃ field-plated Schottky barrier diodes with MOCVD-grown intentionally 1015 cm- 3 doped drift layers,” Journal of Applied Physics 138(18), (2025).DOI
  6. [6]S. Roy, B. Kostroun, Y. Liu, J. Cooke, A. Bhattacharyya, C. Peterson, B. Sensale-Rodriguez, and S. Krishnamoorthy, “Low QCVF 20A/1.4 kV β-Ga₂O₃ Vertical Trench High-k RESURF Schottky Barrier Diode with Turn-on Voltage of 0.5 V,” IEEE Electron Device Letters, (2024).
  7. [7]S. Roy, B. Kostroun, J. Cooke, Y. Liu, A. Bhattacharyya, C. Peterson, B. Sensale-Rodriguez, and S. Krishnamoorthy, “Ultra-low reverse leakage in large area kilo-volt class β-Ga₂O₃ trench Schottky barrier diode with high-k dielectric RESURF,” Applied Physics Letters 123(24), (2023).DOI
  8. [8]“2.34 kV β-Ga₂O₃ vertical trench RESURF Schottky barrier diode with sub-micron fin width | APL Electronic Devices | AIP Publishing,” (n.d.).
  9. [9]Y. Zhang, and J.S. Speck, “Importance of shallow hydrogenic dopants and material purity of ultra-wide bandgap semiconductors for vertical power electron devices,” Semiconductor Science and Technology 35(12), 125018 (2020).DOI
  10. [10]B.J. Baliga, Fundamentals of Power Semiconductor Devices (Springer Science & Business Media, 2010).
  11. [11]J. Wan, H. Wang, C. Zhang, Y. Li, C. Wang, H. Cheng, J. Li, N. Ren, Q. Guo, and K. Sheng, “3.3 kV-class NiO/β-Ga₂O₃ heterojunction diode and its off-state leakage mechanism,” Applied Physics Letters 124(24), (2024).DOI
  12. [12]H.H. Gong, X.H. Chen, Y. Xu, F.-F. Ren, S.L. Gu, and J.D. Ye, “A 1.86-kV double-layered NiO/β-Ga₂O₃ vertical p–n heterojunction diode,” Applied Physics Letters 117(2), (2020).DOI
  13. [13]J.-S. Li, C.-C. Chiang, X. Xia, H.-H. Wan, F. Ren, and S.J. Pearton, “7.5 kV, 6.2 GW cm⁻² NiO/β-Ga₂O₃ vertical rectifiers with on–off ratio greater than 10¹³,” Journal of Vacuum Science & Technology A 41(3), (2023).DOI
  14. [14]J.-S. Li, H.-H. Wan, C.-C. Chiang, T.J. Yoo, F. Ren, H. Kim, and S.J. Pearton, “NiO/Ga₂O₃ Vertical Rectifiers of 7 kV and 1 mm² with 5.5 A Forward Conduction Current,” Crystals 13(12), 1624 (2023).DOI
  15. [15]M. Xiao, B. Wang, J. Spencer, Y. Qin, M. Porter, Y. Ma, Y. Wang, K. Sasaki, M. Tadjer, and Y. Zhang, “NiO junction termination extension for high-voltage (> 3 kV) Ga₂O₃ devices,” Applied Physics Letters 122(18), (2023).DOI
  16. [16]F. Zhou, H. Gong, M. Xiao, Y. Ma, Z. Wang, X. Yu, L. Li, L. Fu, H.H. Tan, Y. Yang, F.-F. Ren, S. Gu, Y. Zheng, H. Lu, R. Zhang, Y. Zhang, and J. Ye, “An avalanche-and-surge robust ultrawide-bandgap heterojunction for power electronics,” Nat Commun 14(1), 4459 (2023).DOI
  17. [17]J.-S. Li, H.-H. Wan, C.-C. Chiang, T.J. Yoo, M.-H. Yu, F. Ren, H. Kim, Y.-T. Liao, and S.J. Pearton, “Breakdown up to 13.5 kV in NiO/β-Ga₂O₃ vertical heterojunction rectifiers,” ECS Journal of Solid State Science and Technology 13(3), 035003 (2024).DOI
  18. [18]Y. Qin, Z. Yang, H. Gong, A.G. Jacobs, J. Spencer, M. Porter, B. Wang, K. Sasaki, C.-H. Lin, and M. Tadjer, “10 kV, 250°C Operational, Enhancement-Mode Ga₂O₃ JFET with Charge-Balance and Hybrid-Drain Designs,” in 2024 IEEE International Electron Devices Meeting (IEDM), (IEEE, 2024), pp. 1–4.DOI
  19. [19]Y. Qin, M. Xiao, M. Porter, Y. Ma, J. Spencer, Z. Du, A.G. Jacobs, K. Sasaki, H. Wang, and M. Tadjer, “10-kV Ga₂O₃ charge-balance Schottky rectifier operational at 200° C,” IEEE Electron Device Letters 44(8), 1268–1271 (2023).DOI
  20. [20]Y. Liu, S.M. Witsell, J.F. Conley, and S. Krishnamoorthy, “Orientation-dependent β-Ga₂O₃ heterojunction diode with atomic layer deposition (ALD) NiO,” Applied Physics Letters 127(12), (2025).DOI
  21. [21]Y. Qin, M. Xiao, R. Zhang, Q. Xie, T. Palacios, B. Wang, Y. Ma, I. Kravchenko, D.P. Briggs, and D.K. Hensley, “1 kV GaN-on-Si quasi-vertical Schottky rectifier,” IEEE Electron Device Letters 44(7), 1052–1055 (2023).DOI
  22. [22]Y. Ma, Y. Qin, M. Porter, J. Spencer, Z. Du, M. Xiao, B. Wang, Y. Wang, A.G. Jacobs, H. Wang, M. Tadjer, and Y. Zhang, “Wide-Bandgap Nickel Oxide with Tunable Acceptor Concentration for Multidimensional Power Devices,” Adv Elect Materials 11(1), 2300662 (2025).
  23. [23]Y. Qin, M. Porter, M. Xiao, Z. Du, H. Zhang, Y. Ma, J. Spencer, B. Wang, Q. Song, and K. Sasaki, “2 kV, 0.7 mΩ• cm² Vertical Ga₂O₃ Superjunction Schottky Rectifier with Dynamic Robustness,” in 2023 International Electron Devices Meeting (IEDM), (IEEE, 2023), pp. 1–4.DOI
  24. [24]M. Xiao, Y. Ma, Z. Du, Y. Qin, K. Liu, K. Cheng, F. Udrea, A. Xie, E. Beam, and B. Wang, “First demonstration of vertical superjunction diode in GaN,” in 2022 International Electron Devices Meeting (IEDM), (IEEE, 2022), pp. 35–6.DOI
  25. [25]K. Egbo, E.M. Garrity, W.A. Callahan, C. Chae, C.-W. Lee, B. Tellekamp, J. Hwang, V. Stevanovic, and A. Zakutayev, “NiGa₂O₄ interfacial layers in NiO/Ga₂O₃ heterojunction diodes at high temperature,” Appl. Phys. Lett. 124(17), 173512 (2024).arxiv.org/abs/2401.06924
  26. [26]D.S. Yu, L. Meng, V.G. Tripathi, V. Vangiparuk, C. Chae, J. Hwang, and H. Zhao, “Metal–organic chemical vapor deposition of p-type NiO and NiO/β-Ga₂O₃ PN diodes,” APL Electronic Devices 1(4), (2025).DOI
  27. [27]M.T. Greiner, M.G. Helander, W.-M. Tang, Z.-B. Wang, J. Qiu, and Z.-H. Lu, “Universal energy-level alignment of molecules on metal oxides,” Nature Materials 11(1), 76–81 (2012).DOI
  28. [28]S. Ghosh, M. Baral, R. Kamparath, R.J. Choudhary, D.M. Phase, S.D. Singh, and T. Ganguli, “Epitaxial growth and interface band alignment studies of all oxide α-Cr₂O₃/β-Ga₂O₃ pn heterojunction,” Applied Physics Letters 115(6), (2019).DOI
  29. [29]H. Mashiko, T. Oshima, and A. Ohtomo, “Band-gap narrowing in α-(CrₓFe₁₋ₓ)₂O₃ solid-solution films,” Applied Physics Letters 99(24), (2011).
  30. [30]C. Su, H. Zhou, Z. Hu, C. Wang, Y. Hao, and J. Zhang, “1.96 kV p-Cr₂O₃/β-Ga₂O₃ heterojunction diodes with an ideality factor of 1.07,” Appl. Phys. Lett. 126(13), 132104 (2025).DOI
  31. [31]Y. Feng, H. Zhou, J. Ma, H. Fang, X. Zhang, Y. Chen, G. Tian, J. Yuan, R. Peng, S. Xu, Y. Hao, and J. Zhang, “120 A/1.78 kV p-Cr₂O₃/n-β-Ga₂O₃ Heterojunction PN Diodes With Slanted Mesa Edge Termination,” IEEE Electron Device Letters 46(10), 1705–1708 (2025).DOI
  32. [32]W.A. Callahan, K. Egbo, C.-W. Lee, D. Ginley, R. O’Hayre, and A. Zakutayev, “Reliable operation of Cr₂O₃:Mg/ β-Ga₂O₃ p–n heterojunction diodes at 600 °C,” Appl. Phys. Lett. 124(15), 153504 (2024).DOI
  33. [33]Y. Liu, S. Roy, C. Peterson, A. Bhattacharyya, and S. Krishnamoorthy, “Ultra-low reverse leakage NiOₓ/β-Ga₂O₃ heterojunction diode achieving breakdown voltage> 3 kV with plasma etch field-termination,” AIP Advances 15(1), (2025).DOI
  34. [34]C.G. Van De Walle, and J. Neugebauer, “Universal alignment of hydrogen levels in semiconductors, insulators and solutions,” Nature 423(6940), 626–628 (2003).pubmed.ncbi.nlm.nih.gov/12789334
  35. [35]W. Kohn, and L.J. Sham, “Self-Consistent Equations Including Exchange and Correlation Effects,” Phys. Rev. 140(4A), A1133–A1138 (1965).DOI
  36. [36]J. Heyd, G.E. Scuseria, and M. Ernzerhof, “Erratum: ‘Hybrid functionals based on a screened Coulomb potential’ [J. Chem. Phys. 118, 8207 (2003)],” The Journal of Chemical Physics 124(21), 219906 (2006).
  37. [37]P.E. Blöchl, “Projector augmented-wave method,” Phys. Rev. B 50(24), 17953–17979 (1994).pubmed.ncbi.nlm.nih.gov/9976227
  38. [38]G. Kresse, and D. Joubert, “From ultrasoft pseudopotentials to the projector augmented-wave method,” Phys. Rev. B 59(3), 1758–1775 (1999).DOI
  39. [39]G. Kresse, and J. Furthmüller, “Efficient iterative schemes for ab initio total-energy calculations using a plane-wave basis set,” Phys. Rev. B 54(16), 11169–11186 (1996).pubmed.ncbi.nlm.nih.gov/9984901
  40. [44]A. Fiedler, R. Schewski, Z. Galazka, and K. Irmscher, “Static dielectric constant of β-Ga2O3 perpendicular to the principal planes (100),(010), and (001),” ECS Journal of Solid State Science and Technology 8(7), Q3083 (2019).
  41. [45]S. Roy, A. Bhattacharyya, C. Peterson, and S. Krishnamoorthy, “2.1 kV (001)-β-Ga2O3 vertical Schottky barrier diode with high-k oxide field plate,” Applied Physics Letters 122(15), (2023).DOI
  42. [46]A. Jain, S.P. Ong, G. Hautier, W. Chen, W.D. Richards, S. Dacek, S. Cholia, D. Gunter, D. Skinner, G. Ceder, and K.A. Persson, “Commentary: The Materials Project: A materials genome approach to accelerating materials innovation,” APL Mater. 1(1), 011002 (2013).DOI

Paper details

vlnc:W_pvgy2yjf
Version
v1 · latest
Published
Fresh — added to the Hub within the last 30 days
Added
License
CC BY 4.0
Usage

views · 0

downloads · 0

A view counts once per browser per day, a download each time the PDF is requested.

  • Physics and Astronomy

Not recorded for this paper

View statement
Looking for related papers…
Contents