Epitaxial growth of WO3 on r-plane sapphire by hot-filament metal-oxide deposition using CO2 as a precursor
Abstract
The deposition of epitaxial films of WO3 by hot-filament metal-oxide deposition using CO2 as a precursor was demonstrated. The films were obtained at a low growth rate of 0.25 nm/min. The optical properties of the film were assessed by variable-angle spectroscopic ellipsometry, indicating transparency across the visible spectrum and high absorption above 3 eV.
Introduction
Tungsten trioxide, denoted with is a versatile multifunctional material with a large compositional homogeneity ranges, and a variety of crystal structures.[1, 2] The properties of interest range from semiconducting behavior with tunable bandgap, thermochromicity[3], electrochromicity[3, 4], photochromicity[5], ferroelectricity[6], superconductivity, gas detection[7, 8, 9] and template for transition metal dichalcogenide growth[10]. Synthesis of has been achieved by a range of physical[7, 8, 11, 12, 13, 14, 15, 16, 17, 18, 19, 20] and chemical[6, 9, 10, 21, 22, 23, 24, 25, 26] vapor deposition techniques. One common approach to the synthesis of is the hot-filament metal oxide deposition (HFMOD) method.[11, 12, 17, 18, 19, 20] The method relies on the oxidation[27, 28, 29, 30] of a hot tungsten wire by flowing [17, 18], [19] or air[11, 12, 17, 20], and on the volatility of the oxides formed.[31]
Here, we instead use as oxidizing species. has long been known as an oxidizing agent of W, for example in reducing the lifetime of tungsten filaments in incandescent lamps[32, 33] and in gas sensing[28]. Besides the advantage of upcycling a major greenhouse gas into valuable materials, is a much milder oxidizer[28] than or . Furthermore, the formation of carbon monoxide (CO) as a byproduct of oxidation of the wires is expected to provide an additional means to tune the composition as it can act as a reducing agent for . This role of CO has been demonstrated in the case of the molybdenum oxides[34], and offers a means of engineering the composition and ultimately the properties of the deposited tungsten oxides. Thus, we here demonstrate epitaxial growth of orthorhombic (-) or monoclinic (-) on r-plane sapphire by HFMOD using as oxidizing gas.
Experimental details
Tungsten oxide thin films were deposited onto r-plane sapphire substrates (-(012), Alineason) in a hot-filament CVD (HFCVD) reactor (Blue Wave Semiconductors BWI 1000 HFCVD) by the reaction of tungsten (2 wires, 0.5-mm diameter, 8-cm long, 99.95% purity) with (99.998% purity). The wires were placed at an average distance of 25 mm from the substrates.
The substrates were sonicated in acetone, isopropanol, and deionized water for 5 min each, then blow-dried using and loaded in an alumina crucible into a crucible furnace. The substrates were annealed in ambient air at 1000 °C for 60 min, with a temperature ramp-up of 5.4 °C/min and a passive cooldown. The substrates were stored in air no longer than three days.
Prior to loading into the HFCVD chamber, the substrates were sonicated once more in acetone and isopropanol for 5 min each, blow-dried using . The base pressure of the system before deposition was Pa (3.0 Torr). The depositions were run using 10 SCCM , resulting in a pressure of Pa (5.4 Torr), at a substrate temperature of 450 °C, for 30-120 min, and with the substrate rotating at a speed of 12.5 rpm. Argon (Ar, 99.999%) was used at the same partial pressure of Pa as a substitute to to dismiss the role of impurities (, residual ) as potential oxidizers. The total current through the filaments was 35 A (17.5 A per filament). The corresponding filament temperature was estimated using the following equation:
where is the temperature of the wire, is the room temperature, is the power dissipated as heat by a resistor, is the emissivity of tungsten which we assumed constant and equal to 0.46 [35], is the Stefan-Boltzmann constant, is the total emitting area, is the total current running through the filaments, is the radius of a filament and the number of identical filaments. The dependence of the resistivity of tungsten in the range 2000 to 3600 K is given by[36]:
which after 6 iterations of equations (1) and (2) converges to K (1947 °C).
X-ray diffraction (XRD) was measured using Cu K radiation. XRD scans were recorded on a PANalytical Empyrean diffractometer with the integrated module iCore (Bragg-Brentano HD graded mirror with 0.8° acceptance angle, 0.03 rad Soller slits, 0.5° divergence slit at a sample distance of 96 mm) on the primary side and the integrated module dCore (17 mm anti-scatter slit, 0.02 rad Soller slits, 0.28° Parallel plate collimator) and PICel3D-Medipix3 detector on the secondary side. GID (Glancing incidence glancing exit diffraction) scans and X-ray pole figure were recorded on a X’Pert MRD diffractometer. A capillary lens with cross-slits was used on the primary side and a 0.18° parallel plate collimator and proportional detector were used on the secondary side, the cross-slits were set to mm for pole figure measurement and mm for GID measurements.
Variable-angle spectroscopic ellipsometry (VASE, RC2-XI Woollam) was used to evaluate the thickness and optical properties of the deposited films. The measurements were performed at incident angles of 50°, 55° and 60° of the range 0.73-5.9 eV. The data was modelled and fit using the CompleteEASE software (6.51).
Results and discussion
Figure 1(a) shows scans from films deposited with for 30 min and 120 min, and for comparison films deposited with pure Ar. The XRD scan from the film deposited with for 30 min exhibits distinct Laue fringes (Figure 1(b)), meaning that films of high crystalline quality are obtained. The fringes for the films deposited for 120 min are difficult to resolve because of their higher thickness of 30 nm, as measured by ellipsometry, corresponding to an average growth rate of 0.25 nm/min.

Figure 1. (a) Extended scans of films deposited on sapphire with for 30 min, 120 min, and without (Ar). (b) Close-up around the tungsten oxide 002 peak
The in Figure 1 and S1 showed a family of peak that is consistent with the planes of several phases of tungsten oxide, namely the monoclinic -, the orthorhombic -, the high-temperature monoclinic phase, and the tetragonal phase.[2] No reflections besides the ones of the substrate are observed when substituting by Ar with a similar impurity level. Indicating that is the main oxidizing species in the process. The asymmetry of the peak is similar to the one reported by other authors for -[14] and tetragonal [8] on r-cut sapphire and may originate from the relaxation of the film.
To get more insight into the symmetry of the phase, GID patterns and pole figures were recorded. The azimuth angle was set to zero for the scan aligned with the -AlO[110] (or -AlO[2 1\bar{1}0]) direction. GID scans were recorded for , , and (Figure 2), forming two sets of orthogonal scans and for , therefore corresponding to a plane of incidence (assuming the sample perfectly flat). Only the families of planes (with or non-zero) are observed. This confirms the out-of-plane relationship as

Figure 2. GID patterns of the 120 min-deposited sample taken along the [110] direction of sapphire, and rotated by , and and . Low intensity, non-indexed peaks and shoulders match with Kβ radiation.
At and , only the plane families such as (e.g. ) are found, from which we deduce the in-plane relationship to
These epitaxial relationships are the same as those reported for monoclinic or orthorhombic synthesized with other methods[7, 14, 16] and unlike reported in[8, 21] where is also found in-plane.
Even the ‘forbidden’ diffraction peaks from the and families of planes are detected. The presence of both and with similar intensities for both and excludes the formation of high symmetry phases such as cubic and tetragonal while indicating a rotational twinning. Distinguishing between orthorhombic - (Pbcn) and monoclinic - (P2/n) is known to be problematic.[7, 16] The and peak positions match better with the orthorhombic phase than the monoclinic one, one may argue that the influence of the substrate may affect in-plane interplanar distances.
XRD pole figures taken at (Figure 3) confirm the epitaxial and twinned nature of the films. The poles in Figure 3 are distributed as follow: two sharp and weak poles at , two sharp and intense poles at , eight poles at and four broad and weak poles at . The sharp poles correspond to (, ) and the tail of (, ). The eight poles at corresponds to , however, this can be interpreted either as the 122 poles of the orthorhombic phase, which appears as eight due to rotational twinning ( poles, the 212 reflections being extinct) or as the superposition of the 122, , 212 and poles of the monoclinic phase, also resulting in eight poles. The monoclinic case would originate from four rotational twins due to its lower symmetry, however the broadening cause by the superposition is in the order of 1 to 2 degrees, which is lower than the step size of the measurement. Similarly, the poles at are associated either to the 221 poles of the orthorhombic phase or the overlap of the 221 and poles of the monoclinic phase.

Figure 3. Pole figures recorded at . The three set of circles correspond three groups of poles.
The real part of the complex dielectric function obtained from VASE shows an increase from 5.15 at 1 eV to a maximum of about at 4 eV (Figure 4). This matches well the one reported in a recent study[37] ( rising from 6 and reaching a maximum of 12 at 4 eV). The imaginary part of the dielectric function and the absorption coefficient are low across most of the visible spectrum (with ). between 1.7 and 2.6 eV) up to around 3 eV where a sharp increase in absorption is observed. The latter value is consistent with reported value of 2.9 eV for the indirect band gap of stoichiometric .[38]

Figure 4. Optical properties of a 30-nm WO thin film deposited on r-cut sapphire a) real part of the dielectric function, b) imaginary part of the dielectric function, and c) absorption coefficient. The feature at 4.5 eV is a fitting artifact.
Conclusion
We have demonstrated the epitaxial growth of monoclinic or orthorhombic on r-cut sapphire by HFMOD using as a precursor. The out-of-plane epitaxial relationship were and the in-plane epitaxial relationships were either or due to 90°-rotational twining. The optical properties, obtained from spectroscopic ellipsometry measurements, were consistent with stoichiometric .
Acknowledgments
We acknowledge funding from the Swedish Research Council VR under project no. 2025-03680, the Swedish Energy Agency under project no. P2025-03108, and the Knut and Alice Wallenberg foundation through the Wallenberg Academy Fellows program (KAW-2020.0196). We acknowledge Myfab Uppsala. Myfab is funded by the Swedish Research Council (2020-00207) as a national research infrastructure.
References
- [1]Wriedt, H. A. The O-W (oxygen-tungsten) system. Bull. Alloy Phase Diagrams 10, 368–384 (1989).DOI
- [2]Howard, C. J., Luca, V. & Knight, K. S. High-temperature phase transitions in tungsten trioxide - the last word ? High-temperature phase transitions in tungsten trioxide — the last word ? J. Phys. Condens. Matter 14, 377 (2002).
- [3]Goulding, M. R., Thomas, C. B. & HurdItch, R. J. A COMPARISON OF THERMO- AND PHOTO-CHROMIC BEHAVIOUR IN FILMS OF AMORPHOUS WO3. Solid State Commun. 46, 451–453 (1983).DOI
- [4]Yano, M. et al. Electrochromic properties of epitaxial WO3 thin films grown on sapphire substrates. Jpn. J. Appl. Phys. 57, (2018).DOI
- [5]Deb, S. K. A Novel Electrophotographic System. Appl. Opt. 8, 192–195 (1969).pubmed.ncbi.nlm.nih.gov/20076124
- [6]Bakhit, B. et al. Evidence for stabilization of ferroelectricity in WO3 thin films under anisotropic epitaxial strain. (2026) doi:10.1063/5.0317226.DOI
- [7]LeGore, L. J., Greenwood, O. D., Paulus, J. W., Frankel, D. J. & Lad, R. J. Controlled growth of WO3 films. J. Vac. Sci. Technol. A 15, 1223–1227 (1997).DOI
- [8]Moulzolf, S. C., LeGore, L. J. & Lad, R. J. Heteroepitaxial growth of tungsten oxide films on sapphire for chemical gas sensors. Thin Solid Films 400, 56–63 (2001).DOI
- [9]Mattinen, M. et al. Atomic Layer Deposition of Molybdenum and Tungsten Oxide Thin Films Using Heteroleptic Imido-Amidinato Precursors : Process Development , Film Characterization , and Gas Sensing Properties Atomic Layer Deposition of Molybdenum and Tungsten Oxide Thin Film. Chem. Mater. 30, 8690–8701 (2018).DOI
- [10]Cohen, A. et al. Tungsten Oxide Mediated Quasi-van der Waals Epitaxy of WS 2 on Sapphire. ACS Nano 17, 5399–5411 (2023).DOI
- [11]Díaz-Reyes, J.; Dorantes-García, V.; Pérez-Benítez, A.; Balderas-López, J. A. Obtaining of films of tungsten trioxide (WO3) by resistive heating of a tungsten filament. Superf. y vacío 21, 12–17 (2008).
- [12]Shankar, N., Yu, M., Vanka, S. P. & Glumac, N. G. Synthesis of tungsten oxide ( WO 3 ) nanorods using carbon nanotubes as templates by hot filament chemical vapor deposition. 60, 771–774 (2006).DOI
- [13]Kobayashi, Y., Terada, S. & Kubota, K. Epitaxial growth of WO3 thin films on MgO and Al2O3. Thin Solid Films 168, 133–139 (1989).DOI
- [14]A Garg, J., Leake, A. & Barber, Z. H. Epitaxial growth of WO 3 films on SrTiO 3 and sapphire. J. Phys. D Appl. Phys. 33, 1048 (2000).DOI
- [15]Leng, X., Pereiro, J., Strle, J., Bollinger, A. T. & Božović, I. Epitaxial growth of high quality WO3 thin films. APL Mater. 3, 1–6 (2015).DOI
- [16]Yano, M. et al. Growth and crystallographic characterization of molecular beam epitaxial WO 3 and MoO 3 /WO 3 thin films on sapphire substrates. Appl. Surf. Sci. 381, 32–35 (2015).
- [17]Thangala, J. et al. Large-Scale , Hot-Filament-Assisted Synthesis of Tungsten Oxide and Related Transition Metal Oxide Nanowires. 40292, 890–896 (2007).pubmed.ncbi.nlm.nih.gov/17415736
- [18]Lu, D., Liang, B., Ogino, A. & Nagatsu, M. Study of the synthesis of tungsten trioxide nanostructured arrays by tungsten hot filament chemical vapor deposition method and their field emission properties. AIP Adv. 1–7 (2010) doi:10.1116/1.3292599.DOI
- [19]Escalante, G. et al. Correlation between Raman spectra and color of tungsten trioxide (WO3 ) thermally evaporated from a tungsten filament. AIP Adv. 11, 055103 (2021).DOI
- [20]Houweling, Z. S. et al. Growth process conditions of tungsten oxide thin films using hot-wire chemical vapor deposition. Mater. Chem. Phys. 131, 375–386 (2011).DOI
- [21]Tägstöm, P. & Jansson, U. Chemical vapour deposition of epitaxial WO3 films. Thin Solid Films 352, 107–113 (1999).DOI
- [22]Dezelah, C. L. I. et al. Atomic Layer Deposition of Tungsten ( III ) Oxide Thin Films from W 2 ( NMe 2 ) 6 and Water : Precursor-Based Control of Oxidation State in the Thin Film Material. J. Am. Chem. Soc. Am. Chem. Soc. 128, 9638–9639 (2006).
- [23]Ito, A. & Morishita, Y. Selective self-oriented growth of (2 0 0), (0 0 2), and (0 2 0) d-WO3 films via metal-organic chemical vapor deposition. Mater. Lett. 258, 126817 (2020).DOI
- [24]Nishihaya, S. et al. Evolution of Insulator – Metal Phase Transitions in Epitaxial Tungsten Oxide Films during Electrolyte-Gating. Appl. Mater. Interfaces (2016) doi:10.1021/acsami.6b06593.DOI
- [25]Yang, J. et al. Effects of line defects on the electronic and optical properties of strain-engineered WO3 thin films. J. Mater. Chem. C 5, 11694–11699 (2017).DOI
- [26]Mattoni, G., Filipetti, A., Manca, N., Zubko, P. & Caviglia, A. D. Charge doping and large lattice expansion in oxygen-deficient heteroepitaxial WO 3. Phys. Rev. Mater. 2, 053402 (2018).DOI
- [27]Kellett, E. A. & Rogers, S. E. The Structure of Oxide Layers on Tungsten. J. Electrochem. Soc. 110, 502 (1963).DOI
- [28]Abel, W. T., Spencer, J. D. & Bailey, D. M. Hot Filament Method of Determining Oxidizing Gases in High-Purity Gas Streams. Anal. Chem. 37, 1711–1715 (1965).DOI
- [29]Warren, A. & Nylund, A. Oxidation of Tungsten and Tungsten Carbide in Dry and Humid Atmospheres. 14, 345–353 (1996).
- [30]Habainy, J., Iyengar, S., Babu, K. & Lee, Y. Formation of oxide layers on tungsten at low oxygen partial pressures. J. Nucl. Mater. 506, 26–34 (2018).DOI
- [31]Blackburn, B. P. E., Hoch, M. & Johnston, H. L. THE VAPORIZATION OF MOLYBDENUM AND TUNGSTEN OXIDES. J. Phys. Chem. 62, 769–773 (1958).
- [32]Harvey, F. J. High Temperature Oxidation of Tungsten Wires in CO2-Argon Mixtures. Metall. Trans. 5, 35–38 (1974).DOI
- [33]Shaffer, J. W. IMPROVED GETTER FOR INCANDESCENT LAMPS. 9 (1989).
- [34]Wang, L. U., Bu, C., Zhang, G. & Wang, J. Study of the Reduction of Industrial Grade MoO 3 Powders with CO or CO-CO 2 Gases to Prepare. Metall. Trans. B 48, 2047–2056 (2017).
- [35]Larrabee, R. D. Spectral Emissivity of Tungsten. J. Opt. Soc. Am. 49, 619–625 (1959).
- [36]Cezairliyan, A. & McClure, J. L. High-Speed ( Subsecond ) Measurement of Heat Capacity , Electrical Resistivity , and Thermal Radiation Properties of Tungsten in the Range 2000 to 3600 K *. J. Res. Notional Bur. Stand. - A. Phys. Chem. 75A, 283–290 (1971).DOI
- [37]Sekora, D., Mock, A., Korlacki, R., Echeverr, E. M. & Ianno, N. Critical-point model dielectric function analysis of WO 3 thin films deposited by atomic layer deposition techniques. 1–6.DOI
- [38]Iwai, T. Temperature Dependence of the Optical Absorption Edge of Tungsten Trioxide Single Crystal. J. Phys. Soc. Japan 15, 1596 (1960).DOI